Revision as of 21:13, 2 October 2010 view source5 albert square (talk | contribs)Autopatrolled, Administrators68,587 editsm Reverted addition of dubious unsourced content (HG)← Previous edit | Latest revision as of 14:50, 13 November 2024 view source Plantsurfer (talk | contribs)Extended confirmed users40,001 editsm Renamed references using RefRenamernamed citations | ||
Line 1: | Line 1: | ||
{{short description|Fibrous material from trees or other plants}} | |||
{{Redirect|Wooden}} | |||
{{pp-semi-indef|small=yes}} | |||
{{three other uses|the substance|small forests|woodland|wood as a ]|lumber}} | |||
{{pp-move|small=yes}} | |||
{{for-multi|a small forest|Woodland|wood as a commodity|Timber|other uses|Wood (disambiguation)|and|Wooden (disambiguation)}} | |||
{{Use mdy dates|date=December 2011}} | |||
{{Use American English|date=October 2012}}<!--THIS ARTICLE WAS STARTED IN AMERICAN SPELLING. PLEASE KEEP PER WP:ENGVAR--> | |||
{{Annotated image 4 | |||
| caption = | |||
| header =Wood samples | |||
| alt = | |||
| image = 16 wood samples.jpg | |||
| align = right | |||
| image-width = 350 | |||
| width = 350 | |||
| height = 431 | |||
| annot-font-size = 12 | |||
| annot-color =f | |||
| annot-text-align = | |||
| annotations = | |||
{{Annotation|10|90| ] |background-color=#F5DEB3}} | |||
{{Annotation|97|90| ] |background-color=#F5DEB3}} | |||
{{Annotation|184|90| ] |background-color=#F5DEB3}} | |||
{{Annotation|270|90| ] |background-color=#F5DEB3}} | |||
{{Annotation|10|197| ] |background-color=#F5DEB3}} | |||
{{Refimprove|date=September 2008}} | |||
{{Annotation|97|197| ] |background-color=#F5DEB3}} | |||
<!--THIS ARTICLE WAS STARTED IN AMERICAN SPELLING. PLEASE KEEP PER WP:ENGVAR--> | |||
{{Annotation|184|197| ] |background-color=#F5DEB3}} | |||
{{Annotation|270|197| ] |background-color=#F5DEB3}} | |||
{{Annotation|10|304| ] |background-color=#F5DEB3}} | |||
] | |||
{{Annotation|97|304| ] |background-color=#F5DEB3}} | |||
'''Wood''' is a hard, fibrous tissue found in many ]. It has been used for centuries for both ] and as a ] material for several types of living areas such as ]s, known as ]. It is an organic material, a natural ] of ] fibers (which are strong in tension) embedded in a matrix of ] which resists compression. In the strict sense wood is produced as secondary ] in the stems of ]s (and other woody plants). In a living tree it transfers ] and ] to the ] and other growing tissues, and has a support function, enabling woody plants to reach large sizes or to stand up for themselves. Wood may also refer to other plant materials with comparable properties, and to material engineered from wood, or wood chips or fiber. | |||
{{Annotation|184|304| ] |background-color=#F5DEB3}} | |||
{{Annotation|270|304| ] |background-color=#F5DEB3}} | |||
{{Annotation|10|411| ] |background-color=#F5DEB3}} | |||
People have used wood for millennia for many purposes, primarily as a ] or as a ] material for making ]s, ]s, ]s, ], packaging, artworks, and ]. Wood can be dated by ] and in some species by ] to make inferences about when a wooden object was created. The year-to-year variation in tree-ring widths and isotopic abundances gives ] to the prevailing climate at that time.<ref name="Briffa, 2008" >{{cite journal | |||
{{Annotation|97|411| ] |background-color=#F5DEB3}} | |||
|author=Briffa K., et al. | |||
{{Annotation|184|411| ] |background-color=#F5DEB3}} | |||
|year=2008 | |||
{{Annotation|270|411| ] |background-color=#F5DEB3}} | |||
|title=Trends in recent temperature and radial tree growth spanning 2000 years across northwest Eurasia. | |||
}} | |||
|journal=Philosophical Transactions of the Royal Society B: Biological Sciences | |||
'''Wood''' is a structural tissue/material found as '']'' in the ] and roots of ]s and other ]s. It is an ]{{snd}}a natural ] of ] fibers that are strong in tension and embedded in a ] of ] that resists compression. Wood is sometimes defined as only the secondary ] in the stems of trees,<ref>{{cite book|author=Hickey, M.|author2=King, C.|date=2001|title=The Cambridge Illustrated Glossary of Botanical Terms|publisher=Cambridge University Press}}</ref> or more broadly to include the same type of tissue elsewhere, such as in the roots of trees or shrubs. In a living tree, it performs a mechanical-support function, enabling woody plants to grow large or to stand up by themselves. It also conveys water and ]s among the ], other growing tissues, and the roots. Wood may also refer to other plant materials with comparable properties, and to material engineered from wood, ], or ]s. | |||
|issue=363 | |||
|pages=2271–2284 | |||
|doi=10.1098/rstb.2007.2199 | |||
|pmid=18048299 | |||
|volume=363 | |||
|pmc=2606779 | |||
}}</ref> | |||
Wood has been used for thousands of years for ], as a ], for making ]s and ]s, ] and ]. More recently it emerged as a feedstock for the production of purified cellulose and its derivatives, such as ] and ]. | |||
==Formation== | |||
Wood, in the strict sense, is yielded by trees, which increase in ] by the formation, between the existing wood and the inner ], of new woody layers which envelop the entire stem, living branches, and roots. Technically this is known as secondary growth; it is the result of cell division in the vascular cambium, a lateral meristem, and subsequent expansion of the new cells. | |||
As of 2020, the growing stock of ]s worldwide was about 557 billion cubic meters.<ref name="FAO-2020">FAO. 2020. '' {{Webarchive|url=https://web.archive.org/web/20221105155828/https://www.fao.org/3/ca9825en/ca9825en.pdf |date=November 5, 2022 }}.'' Rome.</ref> As an abundant, ]<ref>{{cite web | url=https://www.smithsonianmag.com/smart-news/epa-declares-burning-wood-carbon-neutral-180968880/ | title=The EPA Declared That Burning Wood is Carbon Neutral. It's Actually a Lot More Complicated | access-date=June 3, 2022 | archive-date=June 30, 2021 | archive-url=https://web.archive.org/web/20210630153427/https://www.smithsonianmag.com/smart-news/epa-declares-burning-wood-carbon-neutral-180968880/ | url-status=live }}</ref> renewable resource, woody materials have been of intense interest as a source of renewable energy. In 2008, approximately 3.97 billion cubic meters of wood were harvested.<ref name="FAO-2020" /> Dominant uses were for furniture and building construction.<ref name="Horst-2005">Horst H. Nimz, Uwe Schmitt, Eckart Schwab, Otto Wittmann, Franz Wolf "Wood" in ''Ullmann's Encyclopedia of Industrial Chemistry'' 2005, Wiley-VCH, Weinheim. {{doi|10.1002/14356007.a28_305}}</ref> | |||
=== Growth rings === | |||
Where there are clear seasons, growth can occur in a discrete annual or seasonal pattern, leading to ]s; these can usually be most clearly seen on the end of a log, but are also visible on the other surfaces. If these seasons are annual these growth rings are referred to as annual rings. Where there is no seasonal difference growth rings are likely to be indistinct or absent. | |||
Wood is scientifically studied and researched through the discipline of ], which was initiated since the beginning of the 20th century. | |||
If there are differences within a growth ring, then the part of a growth ring nearest the center of the tree, and formed early in the growing season when growth is rapid, is usually composed of wider elements. It is usually lighter in color than that near the outer portion of the ring, and is known as earlywood or springwood. The outer portion formed later in the season is then known as the latewood or summerwood.<ref> www.farmforestline.com.au</ref> However, there are major differences, depending on the kind of wood (see below). | |||
== |
==History== | ||
] public park in ], ] (October 2006).]] | |||
A knot is a particular type of imperfection in a piece of wood; it will affect the technical properties of the wood, usually for the worse, but may be exploited for artistic effect. In a longitudinally sawn plank, a knot will appear as a roughly circular "solid" (usually darker) piece of wood around which the ] of the rest of the wood "flows" (parts and rejoins). Within a knot, the direction of the wood (grain direction) is up to 90 degrees different from the grain direction of the regular wood. | |||
A 2011 discovery in the ] of ] yielded the earliest known plants to have grown wood, approximately 395 to 400 ].<ref>{{cite news|url=https://www.cbc.ca/news/canada/new-brunswick/n-b-fossils-show-origins-of-wood-1.1052870|title=N.B. fossils show origins of wood|publisher=]|access-date=August 12, 2011|date=August 12, 2011|url-status=live|archive-url=https://web.archive.org/web/20110813012432/http://www.cbc.ca/news/canada/new-brunswick/story/2011/08/12/nb-origins-of-wood-found.html|archive-date=August 13, 2011|df=mdy-all}}</ref><ref>{{cite journal|last1=Philippe Gerrienne|display-authors=etal|title=A Simple Type of Wood in Two Early Devonian Plants|journal=Science|volume=333|issue=6044|pages=837|date=Aug 12, 2011|doi=10.1126/science.1208882|pmid=21836008|bibcode=2011Sci...333..837G|hdl=2268/97121 |s2cid=23513139|url=http://orbi.ulg.ac.be/jspui/handle/2268/97121|hdl-access=free}}{{Dead link|date=October 2022 |bot=InternetArchiveBot |fix-attempted=yes }}</ref> | |||
In the tree a knot is either the base of a side ] or a dormant bud. A knot (when the base of a side branch) is conical in shape (hence the roughly circular cross-section) with the tip at the point in stem diameter at which the plant's ] was located when the branch formed as a bud. | |||
Wood can be dated by ] and in some species by ] to determine when a wooden object was created. | |||
During the development of a tree, the lower limbs often die, but may persist for a time, sometimes years. Subsequent layers of growth of the attaching stem are no longer intimately joined with the dead limb, but are grown around it. Hence, dead branches produce knots which are not attached, and likely to drop out after the tree has been sawn into boards. | |||
People have used wood for thousands of years for many purposes, including as a ] or as a ] material for making ]s, ]s, ]s, ], ], ]s, and ]. Known ]s using wood date back ten thousand years. Buildings like the longhouses in ] Europe were made primarily of wood. | |||
In grading lumber and structural timber, knots are classified according to their form, size, soundness, and the firmness with which they are held in place. This firmness is affected by, among other factors, the length of time for which the branch was dead while the attaching stem continued to grow. | |||
Recent use of wood has been enhanced by the addition of steel and bronze into construction.<ref name="Woods-2017">{{cite web|last1=Woods|first1=Sarah|title=A History of Wood from the Stone Age to the 21st Century|url=http://www.ecobuildingpulse.com/products/a-history-of-wood_o|website=EcoBUILDING|publisher=A Publication of The American Institute of Architects|access-date=March 28, 2017|ref=3|url-status=live|archive-url=https://web.archive.org/web/20170329051421/http://www.ecobuildingpulse.com/products/a-history-of-wood_o|archive-date=March 29, 2017|df=mdy-all}}</ref> | |||
Knots materially affect cracking (known in the US as checking, and the UK as shakes) and warping, ease in working, and cleavability of timber. They are defects which weaken timber and lower its value for structural purposes where strength is an important consideration. The weakening effect is much more serious when timber is subjected to forces perpendicular to the grain and/or ] than where under load along the grain and/or ]. The extent to which knots affect the strength of a ] depends upon their position, size, number, and condition. A knot on the upper side is compressed, while one on the lower side is subjected to tension. If there is a season check in the knot, as is often the case, it will offer little resistance to this tensile stress. Small knots, however, may be located along the neutral plane of a beam and increase the strength by preventing longitudinal ]. Knots in a board or plank are least injurious when they extend through it at right angles to its broadest surface. Knots which occur near the ends of a beam do not weaken it. Sound knots which occur in the central portion one-fourth the height of the beam from either edge are not serious defects.<ref>{{cite book | |||
| last = Record | |||
| first = Samuel J | |||
| title = The Mechanical Properties of Wood | |||
| publisher = J. Wiley & Sons | |||
| date = 1914 | |||
| pages = 165 | |||
| url = http://www.gutenberg.org/etext/12299 | |||
| isbn = B000863N3W}}</ref> | |||
The year-to-year variation in tree-ring widths and isotopic abundances gives ] to the prevailing climate at the time a tree was cut.<ref name="Briffa-2008" >{{cite journal | |||
Knots do not necessarily influence the stiffness of structural timber, this will depend on the size and location. Stiffness and elastic strength are more dependent upon the sound wood than upon localised defects. The breaking strength is very susceptible to defects. Sound knots do not weaken wood when subject to compression parallel to the grain. | |||
|author=Briffa, K. | |||
|date=2008 | |||
|title=Trends in recent temperature and radial tree growth spanning 2000 years across northwest Eurasia | |||
|journal=Philosophical Transactions of the Royal Society B: Biological Sciences | |||
|issue= 1501 | |||
|pages=2271–2284 | |||
|doi=10.1098/rstb.2007.2199 | |||
|pmid=18048299 | |||
|volume=363 | |||
|pmc=2606779 | |||
|last2=Shishov | |||
|first2=V.V. | |||
|last3=Melvin | |||
|first3=T.M. | |||
|last4=Vaganov | |||
|first4=E.A. | |||
|last5=Grudd | |||
|first5=H. | |||
|last6=Hantemirov}}</ref> | |||
==Physical properties== | |||
In some decorative applications, wood with knots may be desirable to add visual interest. In applications where wood is ], such as skirting boards, fascia boards, door frames and ], resins present in the timber may continue to 'bleed' through to the surface of a knot for months or even years after manufacture and show as a yellow or brownish stain. A Knot ] paint or solutuion, correctly applied during preparation, may do much to reduce this problem but it is difficult to control completely, especially when using mass-produced kiln-dried timber stocks. | |||
] in a ] showing idealized vertical and horizontal sections. A new layer of wood is added in each growing season, thickening the stem, existing branches and ]s, to form a ].]] | |||
===Growth rings=== | |||
===Heartwood and sapwood===<!-- This section is linked from ] --> | |||
{{see also|Dendrochronology#Growth rings}} | |||
] branch showing 27 annual growth rings, pale sapwood and dark heartwood, and ] (centre dark spot). The dark radial lines are small knots.]] | |||
Heartwood (or old ]) is wood that, as a result of ], has become more resistant to decay. Tylosis is the deposition of chemical substances (a genetically programmed process). Once heartwood formation is complete, the heartwood is dead. Some uncertainty still exists as to whether heartwood is truly dead, as it can still chemically react to decay organisms, but only once (Shigo 1986, 54). | |||
Wood, in the strict sense, is yielded by ]s, which increase in ] by the formation, between the existing wood and the inner ], of new woody layers which envelop the entire stem, living branches, and roots. This process is known as ]; it is the result of cell division in the ], a lateral meristem, and subsequent expansion of the new cells. These cells then go on to form thickened secondary cell walls, composed mainly of ], ] and ]. | |||
Usually heartwood looks different; in that case it can be seen on a cross-section, usually following the growth rings in shape. Heartwood may (or may not) be much darker than living wood. It may (or may not) be sharply distinct from the sapwood. However, other processes, such as decay, can discolor wood, even in woody plants that do not form heartwood, with a similar color difference, which may lead to confusion. | |||
Where the differences between the seasons are distinct, e.g. ], growth can occur in a discrete annual or seasonal pattern, leading to ]s; these can usually be most clearly seen on the end of a log, but are also visible on the other surfaces. If the distinctiveness between seasons is annual (as is the case in equatorial regions, e.g. ]), these growth rings are referred to as annual rings. Where there is little seasonal difference growth rings are likely to be indistinct or absent. If the bark of the tree has been removed in a particular area, the rings will likely be deformed as the plant overgrows the scar. | |||
Sapwood is the younger, outermost wood; in the growing tree it is living wood, and its principal functions are to conduct water from the ]s to the ] and to store up and give back according to the season the reserves prepared in the leaves. However, by the time they become competent to conduct water, all xylem tracheids and vessels have lost their cytoplasm and the cells are therefore functionally dead. All wood in a tree is first formed as sapwood. The more leaves a tree bears and the more vigorous its growth, the larger the volume of sapwood required. Hence trees making rapid growth in the open have thicker sapwood for their size than trees of the same species growing in dense ]s. Sometimes trees (of species that do form heartwood) grown in the open may become of considerable size, 30 cm or more in diameter, before any heartwood begins to form, for example, in second-growth ], or open-grown ]s. | |||
If there are differences within a growth ring, then the part of a growth ring nearest the center of the tree, and formed early in the growing season when growth is rapid, is usually composed of wider elements. It is usually lighter in color than that near the outer portion of the ring, and is known as earlywood or springwood. The outer portion formed later in the season is then known as the latewood or summerwood.<ref> {{webarchive|url=https://web.archive.org/web/20091212121121/http://farmforestline.com.au/pages/2.1.2.1_wood.html |date=December 12, 2009 }} www.farmforestline.com.au</ref> There are major differences, depending on the kind of wood. If a tree grows all its life in the open and the conditions of ] and site remain unchanged, it will make its most rapid growth in youth, and gradually decline. The annual rings of growth are for many years quite wide, but later they become narrower and narrower. Since each succeeding ring is laid down on the outside of the wood previously formed, it follows that unless a tree materially increases its production of wood from year to year, the rings must necessarily become thinner as the trunk gets wider. As a tree reaches maturity its crown becomes more open and the annual wood production is lessened, thereby reducing still more the width of the growth rings. In the case of forest-grown trees so much depends upon the competition of the trees in their struggle for light and nourishment that periods of rapid and slow growth may alternate. Some trees, such as southern ]s, maintain the same width of ring for hundreds of years. On the whole, as a tree gets larger in diameter the width of the growth rings decreases. | |||
The term ''heartwood'' derives solely from its position and not from any vital importance to the tree. This is evidenced by the fact that a tree can thrive with its heart completely decayed. Some species begin to form heartwood very early in life, so having only a thin layer of live sapwood, while in others the change comes slowly. Thin sapwood is characteristic of such species as ], ], ], ], and ], while in ], ], hickory, ], ], and pine, thick sapwood is the rule. Others never form heartwood. | |||
===Knots=== | |||
There is no definite relation between the annual rings of growth and the amount of sapwood. Within the same species the cross-sectional area of the sapwood is very roughly proportional to the size of the crown of the tree. If the rings are narrow, more of them are required than where they are wide. As the tree gets larger, the sapwood must necessarily become thinner or increase materially in volume. Sapwood is thicker in the upper portion of the trunk of a tree than near the base, because the age and the diameter of the upper sections are less. | |||
<!--] and ] redirect directly here.--> | |||
] | |||
As a tree grows, lower branches often die, and their bases may become overgrown and enclosed by subsequent layers of trunk wood, forming a type of imperfection known as a knot. The dead branch may not be attached to the trunk wood except at its base and can drop out after the tree has been sawn into boards. Knots affect the technical properties of the wood, usually reducing tension strength,<ref>{{cite book |last1=Everett |first1=Alan |last2=Barritt |first2=C. M. H. |title=Materials |date=12 May 2014 |publisher=Routledge |isbn=978-1-317-89327-1 |page=38 |url=https://books.google.com/books?id=ncCOAwAAQBAJ&pg=PT38 |language=en |access-date=March 20, 2023 |archive-date=September 8, 2023 |archive-url=https://web.archive.org/web/20230908234050/https://books.google.com/books?id=ncCOAwAAQBAJ&pg=PT38 |url-status=live }} "Knots, particularly edge and arris knots, reduce strength mainly in tension, but not in resistance to shear and splitting."</ref> but may be exploited for visual effect. In a longitudinally sawn plank, a knot will appear as a roughly circular "solid" (usually darker) piece of wood around which the ] of the rest of the wood "flows" (parts and rejoins). Within a knot, the direction of the wood (grain direction) is up to 90 degrees different from the grain direction of the regular wood. | |||
When a tree is very young it is covered with limbs almost, if not entirely, to the ground, but as it grows older some or all of them will eventually die and are either broken off or fall off. Subsequent growth of wood may completely conceal the stubs which will however remain as knots. No matter how smooth and clear a log is on the outside, it is more or less knotty near the middle. Consequently the sapwood of an old tree, and particularly of a forest-grown tree, will be freer from knots than the inner heartwood. Since in most uses of wood, knots are defects that weaken the timber and interfere with its ease of working and other properties, it follows that a given piece of sapwood, because of its position in the tree, may well be stronger than a piece of heartwood from the same tree. | |||
In the tree a knot is either the base of a side ] or a dormant bud. A knot (when the base of a side branch) is conical in shape (hence the roughly circular cross-section) with the inner tip at the point in stem diameter at which the plant's vascular cambium was located when the branch formed as a bud. | |||
It is remarkable that the inner heartwood of old trees remains as sound as it usually does, since in many cases it is hundreds, and in a few instances thousands, of years old. Every broken limb or root, or deep wound from fire, insects, or falling timber, may afford an entrance for decay, which, once started, may penetrate to all parts of the trunk. The larvae of many insects bore into the trees and their tunnels remain indefinitely as sources of weakness. Whatever advantages, however, that sapwood may have in this connection are due solely to its relative age and position. | |||
In grading ] and structural ], knots are classified according to their form, size, soundness, and the firmness with which they are held in place. This firmness is affected by, among other factors, the length of time for which the branch was dead while the attaching stem continued to grow. | |||
If a tree grows all its life in the open and the conditions of ] and site remain unchanged, it will make its most rapid growth in youth, and gradually decline. The annual rings of growth are for many years quite wide, but later they become narrower and narrower. Since each succeeding ring is laid down on the outside of the wood previously formed, it follows that unless a tree materially increases its production of wood from year to year, the rings must necessarily become thinner as the trunk gets wider. As a tree reaches maturity its crown becomes more open and the annual wood production is lessened, thereby reducing still more the width of the growth rings. In the case of forest-grown trees so much depends upon the competition of the trees in their struggle for light and nourishment that periods of rapid and slow growth may alternate. Some trees, such as southern ]s, maintain the same width of ring for hundreds of years. Upon the whole, however, as a tree gets larger in diameter the width of the growth rings decreases. | |||
] | |||
Different pieces of wood cut from a large tree may differ decidedly, particularly if the tree is big and mature. In some trees, the wood laid on late in the life of a tree is softer, lighter, weaker, and more even-textured than that produced earlier, but in other trees, the reverse applies. This may or may not correspond to heartwood and sapwood. In a large log the sapwood, because of the time in the life of the tree when it was grown, may be inferior in ], ], and toughness to equally sound heartwood from the same log. In a smaller tree, the reverse may be true. | |||
{{blockquote|''Knots materially affect cracking and warping, ease in working, and cleavability of timber. They are defects which weaken timber and lower its value for structural purposes where strength is an important consideration. The weakening effect is much more serious when timber is subjected to forces perpendicular to the grain and/or ] than when under load along the grain and/or ]. The extent to which knots affect the strength of a ] depends upon their position, size, number, and condition. A knot on the upper side is compressed, while one on the lower side is subjected to tension. If there is a season check in the knot, as is often the case, it will offer little resistance to this tensile stress. Small knots may be located along the neutral plane of a beam and increase the strength by preventing longitudinal ]. Knots in a board or plank are least injurious when they extend through it at right angles to its broadest surface. Knots which occur near the ends of a beam do not weaken it. Sound knots which occur in the central portion one-fourth the height of the beam from either edge are not serious defects.''|Samuel J. Record|The Mechanical Properties of Wood<ref name="Record-1914">{{cite book | |||
|last = Record | |||
|first = Samuel J | |||
|title = The Mechanical Properties of Wood | |||
|publisher = J. Wiley & Sons | |||
|year = 1914 | |||
|page = 165 | |||
|url = https://www.gutenberg.org/ebooks/12299 | |||
|asin = B000863N3W | |||
|asin-tld = co.uk | |||
|access-date = August 28, 2020 | |||
|archive-date = October 18, 2020 | |||
|archive-url = https://web.archive.org/web/20201018011708/http://www.gutenberg.org/ebooks/12299 | |||
|url-status = live | |||
}}</ref>}} | |||
Knots do not necessarily influence the stiffness of structural timber; this will depend on the size and location. Stiffness and elastic strength are more dependent upon the sound wood than upon localized defects. The breaking strength is very susceptible to defects. Sound knots do not weaken wood when subject to compression parallel to the grain. | |||
==Hard and soft woods== | |||
There is a strong relationship between the properties of wood and the properties of the particular tree that yielded it. For every tree species there is a range of density for the wood it yields. There is a rough correlation between density of a wood and its strength (mechanical properties). For example, while ] is a medium-dense hardwood which is excellent for fine furniture crafting, ] is light, making it useful for ] building. The densest wood may be ]. | |||
In some decorative applications, wood with knots may be desirable to add visual interest. In applications where wood is ], such as skirting boards, fascia boards, door frames and furniture, resins present in the timber may continue to 'bleed' through to the surface of a knot for months or even years after manufacture and show as a yellow or brownish stain. A knot ] paint or solution (knotting), correctly applied during preparation, may do much to reduce this problem but it is difficult to control completely, especially when using mass-produced kiln-dried timber stocks. | |||
It is common to classify wood as either ] or ]. The wood from ] (e.g. pine) is called softwood, and the wood from ] (usually broad-leaved trees, e.g. oak) is called hardwood. These names are a bit misleading, as hardwoods are not necessarily hard, and softwoods are not necessarily soft. The well-known balsa (a hardwood) is actually softer than any commercial softwood. Conversely, some softwoods (e.g. ]) are harder than many hardwoods. | |||
===Heartwood and sapwood===<!-- ] and ] redirect here --> | |||
] products have properties that usually differ from those of natural timbers. (see below) | |||
{{Redirect|Heartwood}} | |||
{{Redirect|Sapwood|the missile also called "SS-6 Sapwood"|R7 Semyorka}} | |||
{{see also|Trunk (botany)}} | |||
] branch showing 27 annual growth rings, pale sapwood, dark heartwood, and ] (center dark spot). The dark radial lines are small knots.]] | |||
'''Heartwood''' (or duramen<ref name="Britannica-1911">{{Cite EB1911|wstitle=Duramen|volume=8|page=692|short=y}}</ref>) is wood that as a result of a naturally occurring chemical transformation has become more resistant to decay. Heartwood formation is a genetically programmed process that occurs spontaneously. Some uncertainty exists as to whether the wood dies during heartwood formation, as it can still chemically react to decay organisms, but only once.<ref>Shigo, Alex. (1986) ''A New Tree Biology Dictionary''. Shigo and Trees, Associates. {{ISBN|0-943563-12-7}}</ref> | |||
The term ''heartwood'' derives solely from its position and not from any vital importance to the tree. This is evidenced by the fact that a tree can thrive with its heart completely decayed. Some species begin to form heartwood very early in life, so having only a thin layer of live sapwood, while in others the change comes slowly. Thin sapwood is characteristic of such species as ], ], ], ], and ], while in ], ], ], ], ], and pine, thick sapwood is the rule.<ref>{{Cite book|url=https://archive.org/details/mechanicalprope02recogoog|page=|quote=The term heartwood derives solely from its position and not from any vital importance to the tree as a tree can thrive with heart completely decayed.|title=The Mechanical Properties of Wood: Including a Discussion of the Factors Affecting the Mechanical Properties, and Methods of Timber Testing|last=Record|first=Samuel James|date=1914|publisher=J. Wiley & Sons, Incorporated|language=en|df=mdy-all}}</ref> Some others never form heartwood. | |||
Heartwood is often visually distinct from the living sapwood and can be distinguished in a cross-section where the boundary will tend to follow the growth rings. For example, it is sometimes much darker. Other processes such as decay or insect invasion can also discolor wood, even in woody plants that do not form heartwood, which may lead to confusion. | |||
'''Sapwood''' (or alburnum<ref name="Alburnum-1911">{{Cite EB1911|wstitle=Alburnum|volume=1|page=516|short=y}}</ref>) is the younger, outermost wood; in the growing tree it is living wood,<ref>Capon, Brian (2005), Botany for Gardeners (2nd ed.), Portland, OR: Timber Publishing, p. 65 {{ISBN|0-88192-655-8}}</ref> and its principal functions are to conduct water from the ]s to the ] and to store up and give back according to the season the reserves prepared in the leaves. By the time they become competent to conduct water, all xylem tracheids and vessels have lost their cytoplasm and the cells are therefore functionally dead. All wood in a tree is first formed as sapwood. The more leaves a tree bears and the more vigorous its growth, the larger the volume of sapwood required. Hence trees making rapid growth in the open have thicker sapwood for their size than trees of the same species growing in dense forests. Sometimes trees (of species that do form heartwood) grown in the open may become of considerable size, {{convert|30|cm|abbr=on}} or more in diameter, before any heartwood begins to form, for example, in second growth ], or open-grown ]s. | |||
] | |||
No definite relation exists between the annual rings of growth and the amount of sapwood. Within the same species the cross-sectional area of the sapwood is very roughly proportional to the size of the crown of the tree. If the rings are narrow, more of them are required than where they are wide. As the tree gets larger, the sapwood must necessarily become thinner or increase materially in volume. Sapwood is relatively thicker in the upper portion of the trunk of a tree than near the base, because the age and the diameter of the upper sections are less. | |||
When a tree is very young it is covered with limbs almost, if not entirely, to the ground, but as it grows older some or all of them will eventually die and are either broken off or fall off. Subsequent growth of wood may completely conceal the stubs which will remain as knots. No matter how smooth and clear a log is on the outside, it is more or less knotty near the middle. Consequently, the sapwood of an old tree, and particularly of a forest-grown tree, will be freer from knots than the inner heartwood. Since in most uses of wood, knots are defects that weaken the timber and interfere with its ease of working and other properties, it follows that a given piece of sapwood, because of its position in the tree, may well be stronger than a piece of heartwood from the same tree. | |||
Different pieces of wood cut from a large tree may differ decidedly, particularly if the tree is big and mature. In some trees, the wood laid on late in the life of a tree is softer, lighter, weaker, and more even textured than that produced earlier, but in other trees, the reverse applies. This may or may not correspond to heartwood and sapwood. In a large log the sapwood, because of the time in the life of the tree when it was grown, may be inferior in ], ], and toughness to equally sound heartwood from the same log. In a smaller tree, the reverse may be true. | |||
===Color=== | ===Color=== | ||
] is distinctively red.]] | |||
In species which show a distinct difference between heartwood and sapwood the natural color of heartwood is usually darker than that of the sapwood, and very frequently the contrast is conspicuous (see section of yew log above). This is produced by deposits in the heartwood of chemical substances, so that a dramatic color difference does not mean a dramatic difference in the mechanical properties of heartwood and sapwood, although there may be a dramatic chemical difference. | |||
In species which show a distinct difference between heartwood and sapwood the natural color of heartwood is usually darker than that of the sapwood, and very frequently the contrast is conspicuous (see section of yew log above). This is produced by deposits in the heartwood of chemical substances, so that a dramatic color variation does not imply a significant difference in the mechanical properties of heartwood and sapwood, although there may be a marked biochemical difference between the two. | |||
Some experiments on very resinous ] specimens indicate an increase in strength, due to the ] which increases the strength when dry. Such resin-saturated heartwood is called "fat lighter". Structures built of fat lighter are almost impervious to rot and ]s, and very flammable. ]s of old longleaf pines are often dug, split into small pieces and sold as kindling for fires. Stumps thus dug may actually remain a century or more since being cut. ] impregnated with crude resin and dried is also greatly increased in strength thereby. | |||
Since the latewood of a growth ring is usually darker in color than the earlywood, this fact may be used in visually judging the density, and therefore the hardness and strength of the material. This is particularly the case with coniferous woods. In ring-porous woods the vessels of the early wood often appear on a finished surface as darker than the denser latewood, though on cross sections of heartwood the reverse is commonly true. Otherwise the color of wood is no indication of strength. | |||
Abnormal discoloration of wood often denotes a diseased condition, indicating unsoundness. The black check in western ] is the result of insect attacks. The reddish-brown streaks so common in hickory and certain other woods are mostly the result of injury by birds. The discoloration is merely an indication of an injury, and in all probability does not of itself affect the properties of the wood. Certain ] impart to wood characteristic colors which thus become symptomatic of weakness. Ordinary sap-staining is due to fungal growth, but does not necessarily produce a weakening effect. | |||
===Water content=== | |||
Water occurs in living wood in three locations, namely: | |||
* in the ]s | |||
* in the ]ic contents of the ] | |||
* as free water in the cell cavities and spaces, especially of the xylem | |||
] | |||
In heartwood it occurs only in the first and last forms. Wood that is thoroughly air-dried (in ] with the moisture content of the air) retains 8–16% of the water in the cell walls, and none, or practically none, in the other forms. Even oven-dried wood retains a small percentage of moisture, but for all except chemical purposes, may be considered absolutely dry. | |||
The general effect of the ] upon the wood substance is to render it softer and more pliable. A similar effect occurs in the softening action of water on rawhide, paper, or cloth. Within certain limits, the greater the water content, the greater its softening effect. The moisture in wood can be measured by several different ]s. | |||
Some experiments on very resinous ] specimens indicate an increase in strength, due to the ] which increases the strength when dry. Such resin-saturated heartwood is called "fat lighter". Structures built of fat lighter are almost impervious to rot and ]s; however they are very flammable. ] of old longleaf pines are often dug, split into small pieces and sold as kindling for fires. Stumps thus dug may actually remain a century or more since being cut. ] impregnated with crude resin and dried is also greatly increased in strength thereby. | |||
] produces a decided increase in the strength of wood, particularly in small specimens. An extreme example is the case of a completely dry ] block 5 cm in section, which will sustain a permanent load four times as great as a green (undried) block of the same size will. | |||
] is distinctively red in color]] | |||
Since the latewood of a growth ring is usually darker in color than the earlywood, this fact may be used in judging the density, and therefore the hardness and strength of the material. This is particularly the case with coniferous woods. In ring-porous woods the vessels of the early wood not infrequently appear on a finished surface as darker than the denser latewood, though on cross sections of heartwood the reverse is commonly true. Except in the manner just stated the color of wood is no indication of strength. | |||
The greatest strength increase due to drying is in the ultimate crushing strength, and strength at ] in endwise compression; these are followed by the modulus of rupture, and stress at elastic limit in cross-bending, while the ] is least affected.<ref name="Record-1914"/> | |||
Abnormal discoloration of wood often denotes a diseased condition, indicating unsoundness. The black check in western ] is the result of insect attacks. The reddish-brown streaks so common in hickory and certain other woods are mostly the result of injury by birds. The discoloration is merely an indication of an injury, and in all probability does not of itself affect the properties of the wood. Certain ] impart to wood characteristic colors which thus become symptomatic of weakness; however an attractive effect known as ] produced by this process is often considered a desirable characteristic. Ordinary sap-staining is due to fungous growth, but does not necessarily produce a weakening effect. | |||
===Structure=== | ===Structure=== | ||
], showing the vessels, rays (white lines) and annual rings: this is intermediate between diffuse-porous and ring-porous, with vessel size declining gradually]] | |||
Wood is a ], ], ] and ] material. It is composed of cells, and the cell walls are composed of micro-fibrils of ] (40% – 50%) and ] (15% – 25%) impregnated with ] (15% – 30%).<ref></ref>]]] | |||
Wood is a ], ], ] and ] (or more specifically, ]) material. It consists of cells, and the cell walls are composed of micro-fibrils of ] (40–50%) and ] (15–25%) impregnated with ] (15–30%).<ref>{{cite web|url=http://treetesting.com/wood_properties_growth_and_structure.htm|title=Wood Properties Growth and Structure 2015|work=treetesting.com|url-status=live|archive-url=https://web.archive.org/web/20160313044617/http://treetesting.com/wood_properties_growth_and_structure.htm|archive-date=March 13, 2016|df=mdy-all}}</ref> | |||
], ]]] | |||
In coniferous or softwood species the wood cells are mostly of one kind, ]s, and as a result the material is much more uniform in structure than that of most |
In coniferous or ] species the wood cells are mostly of one kind, ]s, and as a result the material is much more uniform in structure than that of most ]s. There are no vessels ("pores") in coniferous wood such as one sees so prominently in oak and ash, for example. | ||
The structure of hardwoods is more complex.<ref> |
The structure of hardwoods is more complex.<ref>{{cite web|url=https://nationalvetcontent.edu.au/alfresco/d/d/workspace/SpacesStore/b2f0fcee-47cb-4650-b248-f533d73d5428/13_05/toolbox13_05/unit9_selecting_timber/section2_characteristics/lesson2_hardwood.htm|title=Timber Plus Toolbox, Selecting timber, Characteristics of timber, Structure of hardwoods|work=nationalvetcontent.edu.au|url-status=dead|archive-url=https://web.archive.org/web/20140810184152/https://nationalvetcontent.edu.au/alfresco/d/d/workspace/SpacesStore/b2f0fcee-47cb-4650-b248-f533d73d5428/13_05/toolbox13_05/unit9_selecting_timber/section2_characteristics/lesson2_hardwood.htm|archive-date=August 10, 2014|df=mdy-all}}</ref> The water conducting capability is mostly taken care of by ]: in some cases (oak, chestnut, ash) these are quite large and distinct, in others (], ], ]) too small to be seen without a hand lens. In discussing such woods it is customary to divide them into two large classes, ''ring-porous'' and ''diffuse-porous''.<ref name="Sperry-1994">{{cite journal |last=Sperry |first=John S. |author2=Nichols, Kirk L. |author3=Sullivan, June E. |author4=Eastlack, Sondra E. |title=Xylem Embolism in ring-porous, diffuse-porous, and coniferous trees of Northern Utah and Interior Alaska |journal=Ecology |date=1994 |volume=75 |issue=6 |pages=1736–1752 |jstor=1939633 |doi=10.2307/1939633 |bibcode=1994Ecol...75.1736S |url=http://bioweb.biology.utah.edu/sperry/publications/Sperry%20et%20al.%201994%20Ecology.pdf |access-date=November 30, 2018 |archive-date=August 10, 2017 |archive-url=https://web.archive.org/web/20170810100919/http://bioweb.biology.utah.edu/sperry/publications/Sperry%20et%20al.%201994%20Ecology.pdf |url-status=dead }}</ref> | ||
In ring-porous species, such as ash, black locust, ], chestnut, ], hickory, ], and oak,<ref name="Sperry-1994"/> the larger vessels or pores (as cross sections of vessels are called) are localized in the part of the growth ring formed in spring, thus forming a region of more or less open and porous tissue. The rest of the ring, produced in summer, is made up of smaller vessels and a much greater proportion of wood fibers. These fibers are the elements which give strength and toughness to wood, while the vessels are a source of weakness.<ref>{{cite book |last1=Record |first1=Samuel James |title=The Mechanical Properties of Wood, Including a Discussion of the Factors Affecting the Mechanical Properties, and Methods of Timber Testing |date=1914 |publisher=J. Wiley & sons, Incorporated |url=https://books.google.com/books?id=IbjPAAAAMAAJ&pg=PA44 |language=en |access-date=March 20, 2023 |archive-date=September 8, 2023 |archive-url=https://web.archive.org/web/20230908234053/https://books.google.com/books?id=IbjPAAAAMAAJ&pg=PA44 |url-status=live }}</ref> | |||
], showing the vessels, rays (white lines) and annual rings: this is intermediate between diffuse-porous and ring-porous, with vessel size declining gradually]] | |||
In diffuse-porous woods the pores are evenly sized so that the water conducting capability is scattered throughout the growth ring instead of being collected in a band or row. Examples of this kind of wood are ], ], buckeye, maple, poplar, and willow. Some species, such as ] and ], are on the border between the two classes, forming an intermediate group. | |||
In diffuse-porous woods the pores are evenly sized so that the water conducting capability is scattered throughout the growth ring instead of being collected in a band or row. Examples of this kind of wood are ],<ref name="Sperry-1994"/> ],<ref name="SJRecord-1914">{{cite book|author=Samuel James Record|title=The mechanical properties of wood, including a discussion of the factors affecting the mechanical properties, and methods of timber testing|url=https://archive.org/details/mechanicalprope01recogoog|year=1914|publisher=J. Wiley & sons, inc.|pages=–|df=mdy-all}}</ref> ],<ref name="Sperry-1994"/> buckeye, maple, ], and the '']'' species such as aspen, cottonwood and poplar.<ref name="Sperry-1994"/> Some species, such as ] and ], are on the border between the two classes, forming an intermediate group.<ref name="SJRecord-1914"/> | |||
==== Earlywood and latewood in softwood ==== | |||
]]] | |||
In temperate softwoods there often is a marked difference between latewood and earlywood. The latewood will be denser than that formed early in the season. When examined under a microscope the cells of dense latewood are seen to be very thick-walled and with very small cell cavities, while those formed first in the season have thin walls and large cell cavities. The strength is in the walls, not the cavities. Hence the greater the proportion of latewood the greater the density and strength. In choosing a piece of pine where strength or stiffness is the important consideration, the principal thing to observe is the comparative amounts of earlywood and latewood. The width of ring is not nearly so important as the proportion and nature of the latewood in the ring. | |||
===Earlywood and latewood=== | |||
If a heavy piece of pine is compared with a lightweight piece it will be seen at once that the heavier one contains a larger proportion of latewood than the other, and is therefore showing more clearly demarcated growth rings. In ]s there is not much contrast between the different parts of the ring, and as a result the wood is very uniform in texture and is easy to work. In ], on the other hand, the latewood is very dense and is deep-colored, presenting a very decided contrast to the soft, straw-colored earlywood. | |||
====In softwood==== | |||
It is not only the proportion of latewood, but also its quality, that counts. In specimens that show a very large proportion of latewood it may be noticeably more porous and weigh considerably less than the latewood in pieces that contain but little. One can judge comparative density, and therefore to some extent strength, by visual inspection. | |||
]]] | |||
In temperate softwoods, there often is a marked difference between latewood and earlywood. The latewood will be denser than that formed early in the season. When examined under a microscope, the cells of dense latewood are seen to be very thick-walled and with very small cell cavities, while those formed first in the season have thin walls and large cell cavities. The strength is in the walls, not the cavities. Hence the greater the proportion of latewood, the greater the density and strength. In choosing a piece of pine where strength or stiffness is the important consideration, the principal thing to observe is the comparative amounts of earlywood and latewood. The width of ring is not nearly so important as the proportion and nature of the latewood in the ring. | |||
If a heavy piece of pine is compared with a lightweight piece it will be seen at once that the heavier one contains a larger proportion of latewood than the other, and is therefore showing more clearly demarcated growth rings. In ] there is not much contrast between the different parts of the ring, and as a result the wood is very uniform in texture and is easy to work. In ], on the other hand, the latewood is very dense and is deep-colored, presenting a very decided contrast to the soft, straw-colored earlywood. | |||
] tree]] | |||
No satisfactory explanation can as yet be given for the exact mechanisms determining the formation of earlywood and latewood. Several factors may be involved. In conifers, at least, rate of growth alone does not determine the proportion of the two portions of the ring, for in some cases the wood of slow growth is very hard and heavy, while in others the opposite is true. The quality of the site where the tree grows undoubtedly affects the character of the wood formed, though it is not possible to formulate a rule governing it. In general, however, it may be said that where strength or ease of working is essential, woods of moderate to slow growth should be chosen. | |||
It is not only the proportion of latewood, but also its quality, that counts. In specimens that show a very large proportion of latewood it may be noticeably more porous and weigh considerably less than the latewood in pieces that contain less latewood. One can judge comparative density, and therefore to some extent strength, by visual inspection. | |||
==== Earlywood and latewood in ring-porous woods ==== | |||
] ; tangential view, wide growth rings]] | |||
In ring-porous woods each season's growth is always well defined, because the large pores formed early in the season abut on the denser tissue of the year before. | |||
No satisfactory explanation can as yet be given for the exact mechanisms determining the formation of earlywood and latewood. Several factors may be involved. In conifers, at least, rate of growth alone does not determine the proportion of the two portions of the ring, for in some cases the wood of slow growth is very hard and heavy, while in others the opposite is true. The quality of the site where the tree grows undoubtedly affects the character of the wood formed, though it is not possible to formulate a rule governing it. In general, where strength or ease of working is essential, woods of moderate to slow growth should be chosen. | |||
In the case of the ring-porous hardwoods there seems to exist a pretty definite relation between the rate of growth of timber and its properties. This may be briefly summed up in the general statement that the more rapid the growth or the wider the rings of growth, the heavier, harder, stronger, and stiffer the wood. This, it must be remembered, applies only to ring-porous woods such as oak, ash, hickory, and others of the same group, and is, of course, subject to some exceptions and limitations. | |||
====In ring-porous woods==== | |||
In ring-porous woods of good growth it is usually the latewood in which the thick-walled, strength-giving fibers are most abundant. As the breadth of ring diminishes, this latewood is reduced so that very slow growth produces comparatively light, porous wood composed of thin-walled vessels and wood parenchyma. In good oak these large vessels of the earlywood occupy from 6 to 10 per cent of the volume of the log, while in inferior material they may make up 25 per cent or more. The latewood of good oak is dark colored and firm, and consists mostly of thick-walled fibers which form one-half or more of the wood. In inferior oak, this latewood is much reduced both in quantity and quality. Such variation is very largely the result of rate of growth. | |||
]''; tangential view, wide growth rings]] | |||
In ring-porous woods, each season's growth is always well defined, because the large pores formed early in the season abut on the denser tissue of the year before. | |||
In the case of the ring-porous hardwoods, there seems to exist a pretty definite relation between the rate of growth of timber and its properties. This may be briefly summed up in the general statement that the more rapid the growth or the wider the rings of growth, the heavier, harder, stronger, and stiffer the wood. This, it must be remembered, applies only to ring-porous woods such as oak, ash, hickory, and others of the same group, and is, of course, subject to some exceptions and limitations. | |||
Wide-ringed wood is often called "second-growth", because the growth of the young timber in open stands after the old trees have been removed is more rapid than in trees in a closed forest, and in the manufacture of articles where strength is an important consideration such "second-growth" hardwood material is preferred. This is particularly the case in the choice of hickory for handles and ]s. Here not only strength, but toughness and resilience are important. The results of a series of tests on hickory by the U.S. Forest Service show that: | |||
:"The work or shock-resisting ability is greatest in wide-ringed wood that has from 5 to 14 rings per ] (rings 1.8-5 mm thick), is fairly constant from 14 to 38 rings per inch (rings 0.7-1.8 mm thick), and decreases rapidly from 38 to 47 rings per inch (rings 0.5-0.7 mm thick). The strength at maximum load is not so great with the most rapid-growing wood; it is maximum with from 14 to 20 rings per inch (rings 1.3-1.8 mm thick), and again becomes less as the wood becomes more closely ringed. The natural deduction is that wood of first-class mechanical value shows from 5 to 20 rings per inch (rings 1.3-5 mm thick) and that slower growth yields poorer stock. Thus the inspector or buyer of hickory should discriminate against timber that has more than 20 rings per inch (rings less than 1.3 mm thick). Exceptions exist, however, in the case of normal growth upon dry situations, in which the slow-growing material may be strong and tough."<ref name=USforest>U.S. Department of Agriculture, Forest Products Laboratory. ''''. General Technical Report 113. Madison, WI.</ref> | |||
In ring-porous woods of good growth, it is usually the latewood in which the thick-walled, strength-giving fibers are most abundant. As the breadth of ring diminishes, this latewood is reduced so that very slow growth produces comparatively light, porous wood composed of thin-walled vessels and wood parenchyma. In good oak, these large vessels of the earlywood occupy from six to ten percent of the volume of the log, while in inferior material they may make up 25% or more. The latewood of good oak is dark colored and firm, and consists mostly of thick-walled fibers which form one-half or more of the wood. In inferior oak, this latewood is much reduced both in quantity and quality. Such variation is very largely the result of rate of growth. | |||
The effect of rate of growth on the qualities of chestnut wood is summarised by the same authority as follows: | |||
Wide-ringed wood is often called "second-growth", because the growth of the young timber in open stands after the old trees have been removed is more rapid than in trees in a closed forest, and in the manufacture of articles where strength is an important consideration such "second-growth" hardwood material is preferred. This is particularly the case in the choice of hickory for handles and ]s. Here not only strength, but toughness and resilience are important.<ref name="Record-1914"/> | |||
:"When the rings are wide, the transition from spring wood to summer wood is gradual, while in the narrow rings the spring wood passes into summer wood abruptly. The width of the spring wood changes but little with the width of the annual ring, so that the narrowing or broadening of the annual ring is always at the expense of the summer wood. The narrow vessels of the summer wood make it richer in wood substance than the spring wood composed of wide vessels. Therefore, rapid-growing specimens with wide rings have more wood substance than slow-growing trees with narrow rings. Since the more the wood substance the greater the weight, and the greater the weight the stronger the wood, chestnuts with wide rings must have stronger wood than chestnuts with narrow rings. This agrees with the accepted view that sprouts (which always have wide rings) yield better and stronger wood than seedling chestnuts, which grow more slowly in diameter."<ref name=USforest/> | |||
The results of a series of tests on hickory by the U.S. Forest Service show that: | |||
==== Earlywood and latewood in diffuse-porous woods ==== | |||
:"The work or shock-resisting ability is greatest in wide-ringed wood that has from 5 to 14 rings per inch (rings 1.8-5 mm thick), is fairly constant from 14 to 38 rings per inch (rings 0.7–1.8 mm thick), and decreases rapidly from 38 to 47 rings per inch (rings 0.5–0.7 mm thick). The strength at maximum load is not so great with the most rapid-growing wood; it is maximum with from 14 to 20 rings per inch (rings 1.3–1.8 mm thick), and again becomes less as the wood becomes more closely ringed. The natural deduction is that wood of first-class mechanical value shows from 5 to 20 rings per inch (rings 1.3–5 mm thick) and that slower growth yields poorer stock. Thus the inspector or buyer of hickory should discriminate against timber that has more than 20 rings per inch (rings less than 1.3 mm thick). Exceptions exist, however, in the case of normal growth upon dry situations, in which the slow-growing material may be strong and tough."<ref name="USDA_FPL-2007">U.S. Department of Agriculture, Forest Products Laboratory. '' {{webarchive|url=https://web.archive.org/web/20070315214043/http://www.fpl.fs.fed.us/documnts/fplgtr/fplgtr113/fplgtr113.htm |date=March 15, 2007 }}''. General Technical Report 113. Madison, WI.</ref> | |||
The effect of rate of growth on the qualities of chestnut wood is summarized by the same authority as follows: | |||
:"When the rings are wide, the transition from spring wood to summer wood is gradual, while in the narrow rings the spring wood passes into summer wood abruptly. The width of the spring wood changes but little with the width of the annual ring, so that the narrowing or broadening of the annual ring is always at the expense of the summer wood. The narrow vessels of the summer wood make it richer in wood substance than the spring wood composed of wide vessels. Therefore, rapid-growing specimens with wide rings have more wood substance than slow-growing trees with narrow rings. Since the more the wood substance the greater the weight, and the greater the weight the stronger the wood, chestnuts with wide rings must have stronger wood than chestnuts with narrow rings. This agrees with the accepted view that sprouts (which always have wide rings) yield better and stronger wood than seedling chestnuts, which grow more slowly in diameter."<ref name="USDA_FPL-2007"/> | |||
====In diffuse-porous woods==== | |||
In the diffuse-porous woods, the demarcation between rings is not always so clear and in some cases is almost (if not entirely) invisible to the unaided eye. Conversely, when there is a clear demarcation there may not be a noticeable difference in structure within the growth ring. | In the diffuse-porous woods, the demarcation between rings is not always so clear and in some cases is almost (if not entirely) invisible to the unaided eye. Conversely, when there is a clear demarcation there may not be a noticeable difference in structure within the growth ring. | ||
In diffuse-porous woods, as has been stated, the vessels or pores are even-sized, so that the water conducting capability is scattered throughout the ring instead of collected in the earlywood. The effect of rate of growth is, therefore, not the same as in the ring-porous woods, approaching more nearly the conditions in the conifers. In general it may be stated that such woods of medium growth afford stronger material than when very rapidly or very slowly grown. In many uses of wood, total strength is not the main consideration. If ease of working is prized, wood should be chosen with regard to its uniformity of texture and straightness of grain, which will in most cases occur when there is little contrast between the latewood of one season's growth and the earlywood of the next. | In diffuse-porous woods, as has been stated, the vessels or pores are even-sized, so that the water conducting capability is scattered throughout the ring instead of collected in the earlywood. The effect of rate of growth is, therefore, not the same as in the ring-porous woods, approaching more nearly the conditions in the conifers. In general, it may be stated that such woods of medium growth afford stronger material than when very rapidly or very slowly grown. In many uses of wood, total strength is not the main consideration. If ease of working is prized, wood should be chosen with regard to its uniformity of texture and straightness of grain, which will in most cases occur when there is little contrast between the latewood of one season's growth and the earlywood of the next. | ||
=== |
===Monocots=== | ||
] palm, a monocot, in Java. From this perspective these look not much different from trunks of a ] or ]]] | ] palm, a monocot, in ]. From this perspective these look not much different from trunks of a ] or ]]] | ||
Structural material that |
Structural material that resembles ordinary, "dicot" or conifer timber in its gross handling characteristics is produced by a number of ] plants, and these also are colloquially called wood. Of these, ], botanically a member of the grass family, has considerable economic importance, larger culms being widely used as a building and construction material and in the manufacture of engineered flooring, panels and ]. Another major plant group that produces material that often is called wood are the ]. Of much less importance are plants such as ''],'' '']'' and ''].'' With all this material, the structure and composition of the processed raw material is quite different from ordinary wood. | ||
== |
===Specific gravity=== | ||
The single most revealing property of wood as an indicator of wood quality is ] (Timell 1986),<ref name="Timell-1986">Timell, T.E. 1986. Compression wood in gymnosperms. Springer-Verlag, Berlin. 2150 p.</ref> as both pulp yield and lumber strength are determined by it. Specific gravity is the ratio of the mass of a substance to the mass of an equal volume of water; density is the ratio of a mass of a quantity of a substance to the volume of that quantity and is expressed in mass per unit substance, e.g., grams per milliliter (g/cm<sup>3</sup> or g/ml). The terms are essentially equivalent as long as the metric system is used. Upon drying, wood shrinks and its density increases. Minimum values are associated with green (water-saturated) wood and are referred to as ''basic specific gravity'' (Timell 1986).<ref name="Timell-1986" /> | |||
], ] are among a handful of ]s built entirely of wood, without metal joints. See ] for more details.]] | |||
] occurs in living wood in three conditions, namely: (1) in the ]s, (2) in the ]ic contents of the ], and (3) as free water in the cell cavities and spaces. In heartwood it occurs only in the first and last forms. Wood that is thoroughly air-dried retains from 8-16% of water in the cell walls, and none, or practically none, in the other forms. Even oven-dried wood retains a small percentage of moisture, but for all except chemical purposes, may be considered absolutely dry. | |||
The U.S. ] lists a variety of ways to define specific gravity (G) and density (ρ) for wood:<ref>{{Cite web |title=Wood Handbook: Chapter 4: Moisture Relations and Physical Properties of Wood |url=https://www.fpl.fs.usda.gov/documnts/fplgtr/fplgtr282/chapter_04_fpl_gtr282.pdf |publisher=U.S. Forest Products Laboratory |access-date=September 10, 2023 |archive-date=December 30, 2023 |archive-url=https://web.archive.org/web/20231230131945/https://www.fpl.fs.usda.gov/documnts/fplgtr/fplgtr282/chapter_04_fpl_gtr282.pdf |url-status=live }}</ref> | |||
The general effect of the water content upon the wood substance is to render it softer and more pliable. A similar effect of common observation is in the softening action of water on paper or ]. Within certain limits, the greater the water content, the greater its softening effect. | |||
{| class="wikitable" | |||
!Symbol | |||
!Mass basis | |||
!Volume basis | |||
|- | |||
|G<sub>0</sub> | |||
|Ovendry | |||
|Ovendry | |||
|- | |||
|G<sub>b</sub> (basic) | |||
|Ovendry | |||
|Green | |||
|- | |||
|G<sub>12</sub> | |||
|Ovendry | |||
|12% MC | |||
|- | |||
|G<sub>x</sub> | |||
|Ovendry | |||
|x% MC | |||
|- | |||
|ρ<sub>0</sub> | |||
|Ovendry | |||
|Ovendry | |||
|- | |||
|ρ<sub>12</sub> | |||
|12% MC | |||
|12% MC | |||
|- | |||
|ρ<sub>x</sub> | |||
|x% MC | |||
|x% MC | |||
|} | |||
The FPL has adopted G<sub>b</sub> and G<sub>12</sub> for specific gravity, in accordance with the ] D2555<ref>{{Cite web |title=Standard Practice for Establishing Clear Wood Strength Values |url=https://www.astm.org/d2555-17a.html |access-date=2023-09-09 |website=www.astm.org |language=en |archive-date=April 1, 2023 |archive-url=https://web.archive.org/web/20230401232343/https://www.astm.org/d2555-17a.html |url-status=live }}</ref> standard. These are scientifically useful, but don't represent any condition that could physically occur. The FPL Wood Handbook also provides formulas for approximately converting any of these measurements to any other. | |||
===Density=== | |||
Drying produces a decided increase in the strength of wood, particularly in small specimens. An extreme example is the case of a completely dry ] block 5 cm in section, which will sustain a permanent load four times as great as that which a green (undried) block of the same size will support.{{Citation needed|date=December 2009}} | |||
{{See also|Janka hardness test}} | |||
The greatest increase due to drying is in the ultimate crushing strength, and strength at ] in endwise compression; these are followed by the modulus of rupture, and stress at elastic limit in cross-bending, while the ] is least affected. | |||
Wood density is determined by multiple growth and physiological factors compounded into "one fairly easily measured wood characteristic" (Elliott 1970).<ref name="Elliott-1970">Elliott, G.K. 1970. Wood density in conifers. Commonwealth For. Bureau, Oxford, U.K., Tech. Commun. 8. 44 p.</ref> | |||
Age, diameter, height, radial (trunk) growth, geographical location, site and growing conditions, ] treatment, and seed source all to some degree influence wood density. Variation is to be expected. Within an individual tree, the variation in wood density is often as great as or even greater than that between different trees (Timell 1986).<ref name="Timell-1986" /> Variation of specific gravity within the ] of a tree can occur in either the horizontal or vertical direction. | |||
Because the specific gravity as defined above uses an unrealistic condition, woodworkers tend to use the "average dried weight", which is a density based on mass at 12% moisture content and volume at the same (ρ<sub>12</sub>). This condition occurs when the wood is at equilibrium moisture content with air at about 65% relative humidity and temperature at 30 °C (86 °F). This density is expressed in units of kg/m<sup>3</sup> or lbs/ft<sup>3</sup>. | |||
===Tables=== | |||
The following tables list the mechanical properties of wood and lumber plant species, including bamboo. See also ] for additional properties. | |||
Wood properties:<ref>{{Cite tech report |first=D.W. |last=Green |first2=J.E. |last2=Winandy |first3=D.E. |last3=Kretschmann |chapter=4. Mechanical Properties of Wood |chapter-url=https://www.fpl.fs.usda.gov/documnts/fplgtr/fplgtr113/ch04.pdf |title=Wood handbook: Wood as an engineering material |publisher=U.S. Department of Agriculture, Forest Service, Forest Products Laboratory |year=1999 |id=FPL–GTR–113 |pages=463 |url=https://www.fs.usda.gov/research/treesearch/5734 |doi=10.2737/FPL-GTR-113|hdl=2027/mdp.39015000158041 |hdl-access=free }}</ref><ref name="pfaf-2019" /> | |||
{|class="wikitable mw-collapsible mw-collapsed sortable" | |||
!'''Common name''' | |||
!'''Scientific name''' | |||
!'''Moisture content''' | |||
!'''Density (kg/m<sup>3</sup>)''' | |||
!'''Compressive strength (megapascals)''' | |||
!'''Flexural strength (megapascals)''' | |||
|- | |||
|Red Alder | |||
|'']'' | |||
|Green | |||
|370 | |||
|20.4 | |||
|45 | |||
|- | |||
|Red Alder | |||
|'']'' | |||
|12.00% | |||
|410 | |||
|40.1 | |||
|68 | |||
|- | |||
|Black Ash | |||
|'']'' | |||
|Green | |||
|450 | |||
|15.9 | |||
|41 | |||
|- | |||
|Black Ash | |||
|'']'' | |||
|12.00% | |||
|490 | |||
|41.2 | |||
|87 | |||
|- | |||
|Blue Ash | |||
|'']'' | |||
|Green | |||
|530 | |||
|24.8 | |||
|66 | |||
|- | |||
|Blue Ash | |||
|'']'' | |||
|12.00% | |||
|580 | |||
|48.1 | |||
|95 | |||
|- | |||
|Green Ash | |||
|'']'' | |||
|Green | |||
|530 | |||
|29 | |||
|66 | |||
|- | |||
|Green Ash | |||
|'']'' | |||
|12.00% | |||
|560 | |||
|48.8 | |||
|97 | |||
|- | |||
|Oregon Ash | |||
|'']'' | |||
|Green | |||
|500 | |||
|24.2 | |||
|52 | |||
|- | |||
|Oregon Ash | |||
|'']'' | |||
|12.00% | |||
|550 | |||
|41.6 | |||
|88 | |||
|- | |||
|White Ash | |||
|'']'' | |||
|Green | |||
|550 | |||
|27.5 | |||
|66 | |||
|- | |||
|White Ash | |||
|'']'' | |||
|12.00% | |||
|600 | |||
|51.1 | |||
|103 | |||
|- | |||
|Bigtooth Aspen | |||
|'']'' | |||
|Green | |||
|360 | |||
|17.2 | |||
|37 | |||
|- | |||
|Bigtooth Aspen | |||
|'']'' | |||
|12.00% | |||
|390 | |||
|36.5 | |||
|63 | |||
|- | |||
|Quaking Aspen | |||
|'']'' | |||
|Green | |||
|350 | |||
|14.8 | |||
|35 | |||
|- | |||
|Quaking Aspen | |||
|'']'' | |||
|12.00% | |||
|380 | |||
|29.3 | |||
|58 | |||
|- | |||
|American Basswood | |||
|'']'' | |||
|Green | |||
|320 | |||
|15.3 | |||
|34 | |||
|- | |||
|American Basswood | |||
|'']'' | |||
|12.00% | |||
|370 | |||
|32.6 | |||
|60 | |||
|- | |||
|American Beech | |||
|'']'' | |||
|Green | |||
|560 | |||
|24.5 | |||
|59 | |||
|- | |||
|American Beech | |||
|'']'' | |||
|12.00% | |||
|640 | |||
|50.3 | |||
|103 | |||
|- | |||
|Paper Birch | |||
|'']'' | |||
|Green | |||
|480 | |||
|16.3 | |||
|44 | |||
|- | |||
|Paper Birch | |||
|'']'' | |||
|12.00% | |||
|550 | |||
|39.2 | |||
|85 | |||
|- | |||
|Sweet Birch | |||
|'']'' | |||
|Green | |||
|600 | |||
|25.8 | |||
|65 | |||
|- | |||
|Sweet Birch | |||
|'']'' | |||
|12.00% | |||
|650 | |||
|58.9 | |||
|117 | |||
|- | |||
|Yellow Birch | |||
|'']'' | |||
|Green | |||
|550 | |||
|23.3 | |||
|57 | |||
|- | |||
|Yellow Birch | |||
|'']'' | |||
|12.00% | |||
|620 | |||
|56.3 | |||
|114 | |||
|- | |||
|Butternut | |||
|'']'' | |||
|Green | |||
|360 | |||
|16.7 | |||
|37 | |||
|- | |||
|Butternut | |||
|'']'' | |||
|12.00% | |||
|380 | |||
|36.2 | |||
|56 | |||
|- | |||
|Black Cherry | |||
|'']'' | |||
|Green | |||
|470 | |||
|24.4 | |||
|55 | |||
|- | |||
|Blach Cherry | |||
|'']'' | |||
|12.00% | |||
|500 | |||
|49 | |||
|85 | |||
|- | |||
|American Chestnut | |||
|'']'' | |||
|Green | |||
|400 | |||
|17 | |||
|39 | |||
|- | |||
|American Chestnut | |||
|'']'' | |||
|12.00% | |||
|430 | |||
|36.7 | |||
|59 | |||
|- | |||
|Balsam Poplar Cottonwood | |||
|'']'' | |||
|Green | |||
|310 | |||
|11.7 | |||
|27 | |||
|- | |||
|Balsam Poplar Cottonwood | |||
|'']'' | |||
|12.00% | |||
|340 | |||
|27.7 | |||
|47 | |||
|- | |||
|Black Cottonwood | |||
|'']'' | |||
|Green | |||
|310 | |||
|15.2 | |||
|34 | |||
|- | |||
|Black Cottonwood | |||
|'']'' | |||
|12.00% | |||
|350 | |||
|31 | |||
|59 | |||
|- | |||
|Eastern Cottonwood | |||
|'']'' | |||
|Green | |||
|370 | |||
|15.7 | |||
|37 | |||
|- | |||
|Eastern Cottonwood | |||
|'']'' | |||
|12.00% | |||
|400 | |||
|33.9 | |||
|59 | |||
|- | |||
|American Elm | |||
|'']'' | |||
|Green | |||
|460 | |||
|20.1 | |||
|50 | |||
|- | |||
|American Elm | |||
|'']'' | |||
|12.00% | |||
|500 | |||
|38.1 | |||
|81 | |||
|- | |||
|Rock Elm | |||
|'']'' | |||
|Green | |||
|570 | |||
|26.1 | |||
|66 | |||
|- | |||
|Rock Elm | |||
|'']'' | |||
|12.00% | |||
|630 | |||
|48.6 | |||
|102 | |||
|- | |||
|Slippery Elm | |||
|'']'' | |||
|Green | |||
|480 | |||
|22.9 | |||
|55 | |||
|- | |||
|Slippery Elm | |||
|'']'' | |||
|12.00% | |||
|530 | |||
|43.9 | |||
|90 | |||
|- | |||
|Hackberry | |||
|'']'' | |||
|Green | |||
|490 | |||
|18.3 | |||
|45 | |||
|- | |||
|Hackberry | |||
|'']'' | |||
|12.00% | |||
|530 | |||
|37.5 | |||
|76 | |||
|- | |||
|Bitternut Hickory | |||
|'']'' | |||
|Green | |||
|600 | |||
|31.5 | |||
|71 | |||
|- | |||
|Bitternut Hickory | |||
|'']'' | |||
|12.00% | |||
|660 | |||
|62.3 | |||
|118 | |||
|- | |||
|Nutmeg Hickory | |||
|'']'' | |||
|Green | |||
|560 | |||
|27.4 | |||
|63 | |||
|- | |||
|Nutmeg Hickory | |||
|'']'' | |||
|12.00% | |||
|600 | |||
|47.6 | |||
|114 | |||
|- | |||
|Pecan Hickory | |||
|'']'' | |||
|Green | |||
|600 | |||
|27.5 | |||
|68 | |||
|- | |||
|Pecan Hickory | |||
|'']'' | |||
|12.00% | |||
|660 | |||
|54.1 | |||
|94 | |||
|- | |||
|Water Hickory | |||
|'']'' | |||
|Green | |||
|610 | |||
|32.1 | |||
|74 | |||
|- | |||
|Water Hickory | |||
|'']'' | |||
|12.00% | |||
|620 | |||
|59.3 | |||
|123 | |||
|- | |||
|Mockernut Hickory | |||
|'']'' | |||
|Green | |||
|640 | |||
|30.9 | |||
|77 | |||
|- | |||
|Mockernut Hickory | |||
|'']'' | |||
|12.00% | |||
|720 | |||
|61.6 | |||
|132 | |||
|- | |||
|Pignut Hickory | |||
|'']'' | |||
|Green | |||
|660 | |||
|33.2 | |||
|81 | |||
|- | |||
|Pignut Hickory | |||
|'']'' | |||
|12.00% | |||
|750 | |||
|63.4 | |||
|139 | |||
|- | |||
|Shagbark Hickory | |||
|'']'' | |||
|Green | |||
|640 | |||
|31.6 | |||
|76 | |||
|- | |||
|Shagbark Hickory | |||
|'']'' | |||
|12.00% | |||
|720 | |||
|63.5 | |||
|139 | |||
|- | |||
|Shellbark Hickory | |||
|'']'' | |||
|Green | |||
|620 | |||
|27 | |||
|72 | |||
|- | |||
|Shellbark Hickory | |||
|'']'' | |||
|12.00% | |||
|690 | |||
|55.2 | |||
|125 | |||
|- | |||
|Honeylocust | |||
|'']'' | |||
|Green | |||
|600 | |||
|30.5 | |||
|70 | |||
|- | |||
|Honeylocust | |||
|'']'' | |||
|12.00% | |||
|600 | |||
|51.7 | |||
|101 | |||
|- | |||
|Black Locust | |||
|'']'' | |||
|Green | |||
|660 | |||
|46.9 | |||
|95 | |||
|- | |||
|Black Locust | |||
|'']'' | |||
|12.00% | |||
|690 | |||
|70.2 | |||
|134 | |||
|- | |||
|Cucumber Tree Magnolia | |||
|'']'' | |||
|Green | |||
|440 | |||
|21.6 | |||
|51 | |||
|- | |||
|Cucumber Tree Magnolia | |||
|'']'' | |||
|12.00% | |||
|480 | |||
|43.5 | |||
|85 | |||
|- | |||
|Southern Magnolia | |||
|'']'' | |||
|Green | |||
|460 | |||
|18.6 | |||
|47 | |||
|- | |||
|Southern Magnolia | |||
|'']'' | |||
|12.00% | |||
|500 | |||
|37.6 | |||
|77 | |||
|- | |||
|Bigleaf Maple | |||
|'']'' | |||
|Green | |||
|440 | |||
|22.3 | |||
|51 | |||
|- | |||
|Bigleaf Maple | |||
|'']'' | |||
|12.00% | |||
|480 | |||
|41 | |||
|74 | |||
|- | |||
|Black Maple | |||
|'']'' | |||
|Green | |||
|520 | |||
|22.5 | |||
|54 | |||
|- | |||
|Black Maple | |||
|'']'' | |||
|12.00% | |||
|570 | |||
|46.1 | |||
|92 | |||
|- | |||
|Red Maple | |||
|'']'' | |||
|Green | |||
|490 | |||
|22.6 | |||
|53 | |||
|- | |||
|Red Maple | |||
|'']'' | |||
|12.00% | |||
|540 | |||
|45.1 | |||
|92 | |||
|- | |||
|Silver Maple | |||
|'']'' | |||
|Green | |||
|440 | |||
|17.2 | |||
|40 | |||
|- | |||
|Silver Maple | |||
|'']'' | |||
|12.00% | |||
|470 | |||
|36 | |||
|61 | |||
|- | |||
|Sugar Maple | |||
|'']'' | |||
|Green | |||
|560 | |||
|27.7 | |||
|65 | |||
|- | |||
|Sugar Maple | |||
|'']'' | |||
|12.00% | |||
|630 | |||
|54 | |||
|109 | |||
|- | |||
|Black Red Oak | |||
|'']'' | |||
|Green | |||
|560 | |||
|23.9 | |||
|57 | |||
|- | |||
|Black Red Oak | |||
|'']'' | |||
|12.00% | |||
|610 | |||
|45 | |||
|96 | |||
|- | |||
|Cherrybark Red Oak | |||
|'']'' | |||
|Green | |||
|610 | |||
|31.9 | |||
|74 | |||
|- | |||
|Cherrybark Red Oak | |||
|'']'' | |||
|12.00% | |||
|680 | |||
|60.3 | |||
|125 | |||
|- | |||
|Laurel Red Oak | |||
|'']'' | |||
|Green | |||
|560 | |||
|21.9 | |||
|54 | |||
|- | |||
|Laurel Red Oak | |||
|'']'' | |||
|12.00% | |||
|630 | |||
|48.1 | |||
|87 | |||
|- | |||
|Northern Red Oak | |||
|'']'' | |||
|Green | |||
|560 | |||
|23.7 | |||
|57 | |||
|- | |||
|Northern Red Oak | |||
|'']'' | |||
|12.00% | |||
|630 | |||
|46.6 | |||
|99 | |||
|- | |||
|Pin Red Oak | |||
|'']'' | |||
|Green | |||
|580 | |||
|25.4 | |||
|57 | |||
|- | |||
|Pin Red Oak | |||
|'']'' | |||
|12.00% | |||
|630 | |||
|47 | |||
|97 | |||
|- | |||
|Scarlet Red Oak | |||
|'']'' | |||
|Green | |||
|600 | |||
|28.2 | |||
|72 | |||
|- | |||
|Scarlet Red Oak | |||
|'']'' | |||
|12.00% | |||
|670 | |||
|57.4 | |||
|120 | |||
|- | |||
|Southern Red Oak | |||
|'']'' | |||
|Green | |||
|520 | |||
|20.9 | |||
|48 | |||
|- | |||
|Southern Red Oak | |||
|'']'' | |||
|12.00% | |||
|590 | |||
|42 | |||
|75 | |||
|- | |||
|Water Red Oak | |||
|'']'' | |||
|Green | |||
|560 | |||
|25.8 | |||
|61 | |||
|- | |||
|Water Red Oak | |||
|'']'' | |||
|12.00% | |||
|630 | |||
|46.7 | |||
|106 | |||
|- | |||
|Willow Red Oak | |||
|'']'' | |||
|Green | |||
|560 | |||
|20.7 | |||
|51 | |||
|- | |||
|Willow Red Oak | |||
|'']'' | |||
|12.00% | |||
|690 | |||
|48.5 | |||
|100 | |||
|- | |||
|Bur White Oak | |||
|'']'' | |||
|Green | |||
|580 | |||
|22.7 | |||
|50 | |||
|- | |||
|Bur White Oak | |||
|'']'' | |||
|12.00% | |||
|640 | |||
|41.8 | |||
|71 | |||
|- | |||
|Chestnut White Oak | |||
|'']'' | |||
|Green | |||
|570 | |||
|24.3 | |||
|55 | |||
|- | |||
|Chestnut White Oak | |||
|'']'' | |||
|12.00% | |||
|660 | |||
|47.1 | |||
|92 | |||
|- | |||
|Live White Oak | |||
|'']'' | |||
|Green | |||
|800 | |||
|37.4 | |||
|82 | |||
|- | |||
|Live White Oak | |||
|'']'' | |||
|12.00% | |||
|880 | |||
|61.4 | |||
|127 | |||
|- | |||
|Overcup White Oak | |||
|'']'' | |||
|Green | |||
|570 | |||
|23.2 | |||
|55 | |||
|- | |||
|Overcup White Oak | |||
|'']'' | |||
|12.00% | |||
|630 | |||
|42.7 | |||
|87 | |||
|- | |||
|Post White Oak | |||
|'']'' | |||
|Green | |||
|600 | |||
|24 | |||
|56 | |||
|- | |||
|Post White Oak | |||
|'']'' | |||
|12.00% | |||
|670 | |||
|45.3 | |||
|91 | |||
|- | |||
|Swamp Chestnut White Oak | |||
|'']'' | |||
|Green | |||
|600 | |||
|24.4 | |||
|59 | |||
|- | |||
|Swamp Chestnut White Oak | |||
|'']'' | |||
|12.00% | |||
|670 | |||
|50.1 | |||
|96 | |||
|- | |||
|Swamp White Oak | |||
|'']'' | |||
|Green | |||
|640 | |||
|30.1 | |||
|68 | |||
|- | |||
|Swamp White Oak | |||
|'']'' | |||
|12.00% | |||
|720 | |||
|59.3 | |||
|122 | |||
|- | |||
|White Oak | |||
|'']'' | |||
|Green | |||
|600 | |||
|24.5 | |||
|57 | |||
|- | |||
|White Oak | |||
|'']'' | |||
|12.00% | |||
|680 | |||
|51.3 | |||
|105 | |||
|- | |||
|Sassafras | |||
|'']'' | |||
|Green | |||
|420 | |||
|18.8 | |||
|41 | |||
|- | |||
|Sassafras | |||
|'']'' | |||
|12.00% | |||
|460 | |||
|32.8 | |||
|62 | |||
|- | |||
|Sweetgum | |||
|'']'' | |||
|Green | |||
|460 | |||
|21 | |||
|49 | |||
|- | |||
|Sweetgum | |||
|'']'' | |||
|12.00% | |||
|520 | |||
|43.6 | |||
|86 | |||
|- | |||
|American Sycamore | |||
|'']'' | |||
|Green | |||
|460 | |||
|20.1 | |||
|45 | |||
|- | |||
|American Sycamore | |||
|'']'' | |||
|12.00% | |||
|490 | |||
|37.1 | |||
|69 | |||
|- | |||
|Tanoak | |||
|'']'' | |||
|Green | |||
|580 | |||
|32.1 | |||
|72 | |||
|- | |||
|Tanoak | |||
|'']'' | |||
|12.00% | |||
|580 | |||
|32.1 | |||
|72 | |||
|- | |||
|Black Tupelo | |||
|'']'' | |||
|Green | |||
|460 | |||
|21 | |||
|48 | |||
|- | |||
|Black Tupelo | |||
|'']'' | |||
|12.00% | |||
|500 | |||
|38.1 | |||
|66 | |||
|- | |||
|Water Tupelo | |||
|'']'' | |||
|Green | |||
|460 | |||
|23.2 | |||
|50 | |||
|- | |||
|Water Tupelo | |||
|'']'' | |||
|12.00% | |||
|500 | |||
|40.8 | |||
|66 | |||
|- | |||
|Black Walnut | |||
|'']'' | |||
|Green | |||
|510 | |||
|29.6 | |||
|66 | |||
|- | |||
|Black Walnut | |||
|'']'' | |||
|12.00% | |||
|550 | |||
|52.3 | |||
|101 | |||
|- | |||
|Black Willow | |||
|'']'' | |||
|Green | |||
|360 | |||
|14.1 | |||
|33 | |||
|- | |||
|Black Willow | |||
|'']'' | |||
|12.00% | |||
|390 | |||
|28.3 | |||
|54 | |||
|- | |||
|Yellow Poplar | |||
|'']'' | |||
|Green | |||
|400 | |||
|18.3 | |||
|41 | |||
|- | |||
|Yellow Poplar | |||
|'']'' | |||
|12.00% | |||
|420 | |||
|38.2 | |||
|70 | |||
|- | |||
|Baldcypress | |||
|'']'' | |||
|Green | |||
|420 | |||
|24.7 | |||
|46 | |||
|- | |||
|Baldcypress | |||
|'']'' | |||
|12.00% | |||
|460 | |||
|43.9 | |||
|73 | |||
|- | |||
|Atlantic White Cedar | |||
|'']'' | |||
|Green | |||
|310 | |||
|16.5 | |||
|32 | |||
|- | |||
|Atlantic White Cedar | |||
|'']'' | |||
|12.00% | |||
|320 | |||
|32.4 | |||
|47 | |||
|- | |||
|Eastern Redcedar | |||
|'']'' | |||
|Green | |||
|440 | |||
|24.6 | |||
|48 | |||
|- | |||
|Eastern Redcedar | |||
|'']'' | |||
|12.00% | |||
|470 | |||
|41.5 | |||
|61 | |||
|- | |||
|Incense Cedar | |||
|'']'' | |||
|Green | |||
|350 | |||
|21.7 | |||
|43 | |||
|- | |||
|Incense Cedar | |||
|'']'' | |||
|12.00% | |||
|370 | |||
|35.9 | |||
|55 | |||
|- | |||
|Northern White Cedar | |||
|'']'' | |||
|Green | |||
|290 | |||
|13.7 | |||
|29 | |||
|- | |||
|Northern White Cedar | |||
|'']'' | |||
|12.00% | |||
|310 | |||
|27.3 | |||
|45 | |||
|- | |||
|Port Orford Cedar | |||
|'']'' | |||
|Green | |||
|390 | |||
|21.6 | |||
|45 | |||
|- | |||
|Port Orford Cedar | |||
|'']'' | |||
|12.00% | |||
|430 | |||
|43.1 | |||
|88 | |||
|- | |||
|Western Redcedar | |||
|'']'' | |||
|Green | |||
|310 | |||
|19.1 | |||
|35.9 | |||
|- | |||
|Western Redcedar | |||
|'']'' | |||
|12.00% | |||
|320 | |||
|31.4 | |||
|51.7 | |||
|- | |||
|Yellow Cedar | |||
|'']'' | |||
|Green | |||
|420 | |||
|21 | |||
|44 | |||
|- | |||
|Yellow Cedar | |||
|'']'' | |||
|12.00% | |||
|440 | |||
|43.5 | |||
|77 | |||
|- | |||
|Coast Douglas Fir | |||
|'']'' | |||
|Green | |||
|450 | |||
|26.1 | |||
|53 | |||
|- | |||
|Coast Douglas Fir | |||
|'']'' | |||
|12.00% | |||
|480 | |||
|49.9 | |||
|85 | |||
|- | |||
|Interior West Douglas Fir | |||
|'']'' | |||
|Green | |||
|460 | |||
|26.7 | |||
|53 | |||
|- | |||
|Interior West Douglas Fir | |||
|'']'' | |||
|12.00% | |||
|500 | |||
|51.2 | |||
|87 | |||
|- | |||
|Interior North Douglas Fir | |||
|'']'' | |||
|Green | |||
|450 | |||
|23.9 | |||
|51 | |||
|- | |||
|Interior North Douglas Fir | |||
|'']'' | |||
|12.00% | |||
|480 | |||
|47.6 | |||
|90 | |||
|- | |||
|Interior South Douglas Fir | |||
|'']'' | |||
|Green | |||
|430 | |||
|21.4 | |||
|47 | |||
|- | |||
|Interior South Douglas Fir | |||
|'']'' | |||
|12.00% | |||
|460 | |||
|43 | |||
|82 | |||
|- | |||
|Balsam Fir | |||
|'']'' | |||
|Green | |||
|330 | |||
|18.1 | |||
|38 | |||
|- | |||
|Balsam Fir | |||
|'']'' | |||
|12.00% | |||
|350 | |||
|36.4 | |||
|63 | |||
|- | |||
|California Red Fir | |||
|'']'' | |||
|Green | |||
|360 | |||
|19 | |||
|40 | |||
|- | |||
|California Red Fir | |||
|'']'' | |||
|12.00% | |||
|380 | |||
|37.6 | |||
|72.4 | |||
|- | |||
|Grand Fir | |||
|'']'' | |||
|Green | |||
|350 | |||
|20.3 | |||
|40 | |||
|- | |||
|Grand Fir | |||
|'']'' | |||
|12.00% | |||
|370 | |||
|36.5 | |||
|61.4 | |||
|- | |||
|Noble Fir | |||
|'']'' | |||
|Green | |||
|370 | |||
|20.8 | |||
|43 | |||
|- | |||
|Noble Fir | |||
|'']'' | |||
|12.00% | |||
|390 | |||
|42.1 | |||
|74 | |||
|- | |||
|Pacific Silver Fir | |||
|'']'' | |||
|Green | |||
|400 | |||
|21.6 | |||
|44 | |||
|- | |||
|Pacific Silver Fir | |||
|'']'' | |||
|12.00% | |||
|430 | |||
|44.2 | |||
|75 | |||
|- | |||
|Subalpine Fir | |||
|'']'' | |||
|Green | |||
|310 | |||
|15.9 | |||
|34 | |||
|- | |||
|Subalpine Fir | |||
|'']'' | |||
|12.00% | |||
|320 | |||
|33.5 | |||
|59 | |||
|- | |||
|White Fir | |||
|'']'' | |||
|Green | |||
|370 | |||
|20 | |||
|41 | |||
|- | |||
|White Fir | |||
|'']'' | |||
|12.00% | |||
|390 | |||
|40 | |||
|68 | |||
|- | |||
|Eastern Hemlock | |||
|'']'' | |||
|Green | |||
|380 | |||
|21.2 | |||
|44 | |||
|- | |||
|Eastern Hemlock | |||
|'']'' | |||
|12.00% | |||
|400 | |||
|37.3 | |||
|61 | |||
|- | |||
|Mountain Hemlock | |||
|'']'' | |||
|Green | |||
|420 | |||
|19.9 | |||
|43 | |||
|- | |||
|Mountain Hemlock | |||
|'']'' | |||
|12.00% | |||
|450 | |||
|44.4 | |||
|79 | |||
|- | |||
|Western Hemlock | |||
|'']'' | |||
|Green | |||
|420 | |||
|23.2 | |||
|46 | |||
|- | |||
|Western Hemlock | |||
|'']'' | |||
|12.00% | |||
|450 | |||
|49 | |||
|78 | |||
|- | |||
|Western Larch | |||
|'']'' | |||
|Green | |||
|480 | |||
|25.9 | |||
|53 | |||
|- | |||
|Western Larch | |||
|'']'' | |||
|12.00% | |||
|520 | |||
|52.5 | |||
|90 | |||
|- | |||
|Eastern White Pine | |||
|'']'' | |||
|Green | |||
|340 | |||
|16.8 | |||
|34 | |||
|- | |||
|Eastern White Pine | |||
|'']'' | |||
|12.00% | |||
|350 | |||
|33.1 | |||
|59 | |||
|- | |||
|Jack Pine | |||
|'']'' | |||
|Green | |||
|400 | |||
|20.3 | |||
|41 | |||
|- | |||
|Jack Pine | |||
|'']'' | |||
|12.00% | |||
|430 | |||
|39 | |||
|68 | |||
|- | |||
|Loblolly Pine | |||
|'']'' | |||
|Green | |||
|470 | |||
|24.2 | |||
|50 | |||
|- | |||
|Loblolly Pine | |||
|'']'' | |||
|12.00% | |||
|510 | |||
|49.2 | |||
|88 | |||
|- | |||
|Lodgepole Pine | |||
|'']'' | |||
|Green | |||
|380 | |||
|18 | |||
|38 | |||
|- | |||
|Lodgepole Pine | |||
|'']'' | |||
|12.00% | |||
|410 | |||
|37 | |||
|65 | |||
|- | |||
|Longleaf Pine | |||
|'']'' | |||
|Green | |||
|540 | |||
|29.8 | |||
|59 | |||
|- | |||
|Longleaf Pine | |||
|'']'' | |||
|12.00% | |||
|590 | |||
|58.4 | |||
|100 | |||
|- | |||
|Pitch Pine | |||
|'']'' | |||
|Green | |||
|470 | |||
|20.3 | |||
|47 | |||
|- | |||
|Pitch Pine | |||
|'']'' | |||
|12.00% | |||
|520 | |||
|41 | |||
|74 | |||
|- | |||
|Pond Pine | |||
|'']'' | |||
|Green | |||
|510 | |||
|25.2 | |||
|51 | |||
|- | |||
|Pond Pine | |||
|'']'' | |||
|12.00% | |||
|560 | |||
|52 | |||
|80 | |||
|- | |||
|Ponderosa Pine | |||
|'']'' | |||
|Green | |||
|380 | |||
|16.9 | |||
|35 | |||
|- | |||
|Ponderosa Pine | |||
|'']'' | |||
|12.00% | |||
|400 | |||
|36.7 | |||
|65 | |||
|- | |||
|Red Pine | |||
|'']'' | |||
|Green | |||
|410 | |||
|18.8 | |||
|40 | |||
|- | |||
|Red Pine | |||
|'']'' | |||
|12.00% | |||
|460 | |||
|41.9 | |||
|76 | |||
|- | |||
|Sand Pine | |||
|'']'' | |||
|Green | |||
|460 | |||
|23.7 | |||
|52 | |||
|- | |||
|Sand Pine | |||
|'']'' | |||
|12.00% | |||
|480 | |||
|47.7 | |||
|80 | |||
|- | |||
|Shortleaf Pine | |||
|'']'' | |||
|Green | |||
|470 | |||
|24.3 | |||
|51 | |||
|- | |||
|Shortleaf Pine | |||
|'']'' | |||
|12.00% | |||
|510 | |||
|50.1 | |||
|90 | |||
|- | |||
|Slash Pine | |||
|'']'' | |||
|Green | |||
|540 | |||
|26.3 | |||
|60 | |||
|- | |||
|Slash Pine | |||
|'']'' | |||
|12.00% | |||
|590 | |||
|56.1 | |||
|112 | |||
|- | |||
|Spruce Pine | |||
|'']'' | |||
|Green | |||
|410 | |||
|19.6 | |||
|41 | |||
|- | |||
|Spruce Pine | |||
|'']'' | |||
|12.00% | |||
|440 | |||
|39 | |||
|72 | |||
|- | |||
|Sugar Pine | |||
|'']'' | |||
|Green | |||
|340 | |||
|17 | |||
|34 | |||
|- | |||
|Sugar Pine | |||
|'']'' | |||
|12.00% | |||
|360 | |||
|30.8 | |||
|57 | |||
|- | |||
|Virginia Pine | |||
|'']'' | |||
|Green | |||
|450 | |||
|23.6 | |||
|50 | |||
|- | |||
|Virginia Pine | |||
|'']'' | |||
|12.00% | |||
|480 | |||
|46.3 | |||
|90 | |||
|- | |||
|Western White Pine | |||
|'']'' | |||
|Green | |||
|360 | |||
|16.8 | |||
|32 | |||
|- | |||
|Western White Pine | |||
|'']'' | |||
|12.00% | |||
|380 | |||
|34.7 | |||
|67 | |||
|- | |||
|Redwood Old Growth | |||
|'']'' | |||
|Green | |||
|380 | |||
|29 | |||
|52 | |||
|- | |||
|Redwood Old Growth | |||
|'']'' | |||
|12.00% | |||
|400 | |||
|42.4 | |||
|69 | |||
|- | |||
|Redwood New Growth | |||
|'']'' | |||
|Green | |||
|340 | |||
|21.4 | |||
|41 | |||
|- | |||
|Redwood New Growth | |||
|'']'' | |||
|12.00% | |||
|350 | |||
|36 | |||
|54 | |||
|- | |||
|Black Spruce | |||
|'']'' | |||
|Green | |||
|380 | |||
|19.6 | |||
|42 | |||
|- | |||
|Black Spruce | |||
|'']'' | |||
|12.00% | |||
|460 | |||
|41.1 | |||
|74 | |||
|- | |||
|Engelmann Spruce | |||
|'']'' | |||
|Green | |||
|330 | |||
|15 | |||
|32 | |||
|- | |||
|Engelmann Spruce | |||
|'']'' | |||
|12.00% | |||
|350 | |||
|30.9 | |||
|64 | |||
|- | |||
|Red Spruce | |||
|'']'' | |||
|Green | |||
|370 | |||
|18.8 | |||
|41 | |||
|- | |||
|Red Spruce | |||
|'']'' | |||
|12.00% | |||
|400 | |||
|38.2 | |||
|74 | |||
|- | |||
|Sitka Spruce | |||
|'']'' | |||
|Green | |||
|330 | |||
|16.2 | |||
|34 | |||
|- | |||
|Sitka Spruce | |||
|'']'' | |||
|12.00% | |||
|360 | |||
|35.7 | |||
|65 | |||
|- | |||
|White Spruce | |||
|'']'' | |||
|Green | |||
|370 | |||
|17.7 | |||
|39 | |||
|- | |||
|White Spruce | |||
|'']'' | |||
|12.00% | |||
|400 | |||
|37.7 | |||
|68 | |||
|- | |||
|Tamarack Spruce | |||
|'']'' | |||
|Green | |||
|490 | |||
|24 | |||
|50 | |||
|- | |||
|Tamarack Spruce | |||
|'']'' | |||
|12.00% | |||
|530 | |||
|49.4 | |||
|80 | |||
|} | |||
Bamboo properties:<ref>{{Cite web|title=What are the mechanical properties of bamboo|url=https://doorstain.com/blog/news/what-are-the-mechanical-properties-of-bamboo/|access-date=2023-08-22|website=www.DoorStain.com|date=August 22, 2023 |archive-date=August 22, 2023|archive-url=https://web.archive.org/web/20230822211225/https://doorstain.com/blog/news/what-are-the-mechanical-properties-of-bamboo/|url-status=live}}</ref><ref name="pfaf-2019">{{Cite web|url=https://pfaf.org/user/Default.aspx|title=PFAF|website=pfaf.org|access-date=2019-11-03|archive-date=October 24, 2019|archive-url=https://web.archive.org/web/20191024204115/https://pfaf.org/user/default.aspx|url-status=live}}</ref> | |||
{|class="wikitable mw-collapsible mw-collapsed sortable" | |||
!'''Common name''' | |||
!'''Scientific name''' | |||
!'''Moisture content''' | |||
!'''Density (kg/m<sup>3</sup>)''' | |||
!'''Compressive strength (megapascals)''' | |||
!'''Flexural strength (megapascals)''' | |||
|- | |||
|Balku bans | |||
|'']'' | |||
|green | |||
| | |||
|45 | |||
|73.7 | |||
|- | |||
|Balku bans | |||
|'']'' | |||
|air dry | |||
| | |||
|54.15 | |||
|81.1 | |||
|- | |||
|Balku bans | |||
|'']'' | |||
|8.5 | |||
|820 | |||
|69 | |||
|151 | |||
|- | |||
|Indian thorny bamboo | |||
|'']'' | |||
|9.5 | |||
|710 | |||
|61 | |||
|143 | |||
|- | |||
|Indian thorny bamboo | |||
|'']'' | |||
| | |||
| | |||
|43.05 | |||
|37.15 | |||
|- | |||
|Nodding Bamboo | |||
|'']'' | |||
|8 | |||
|890 | |||
|75 | |||
|52.9 | |||
|- | |||
|Nodding Bamboo | |||
|'']'' | |||
|87 | |||
| | |||
|46 | |||
|52.4 | |||
|- | |||
|Nodding Bamboo | |||
|'']'' | |||
|12 | |||
| | |||
|85 | |||
|67.5 | |||
|- | |||
|Nodding Bamboo | |||
|'']'' | |||
|88.3 | |||
| | |||
|44.7 | |||
|88 | |||
|- | |||
|Nodding Bamboo | |||
|'']'' | |||
|14 | |||
| | |||
|47.9 | |||
|216 | |||
|- | |||
|Clumping Bamboo | |||
|'']'' | |||
| | |||
| | |||
|45.8 | |||
| | |||
|- | |||
|Clumping Bamboo | |||
|'']'' | |||
|5 | |||
| | |||
|79 | |||
|80 | |||
|- | |||
|Clumping Bamboo | |||
|'']'' | |||
|20 | |||
| | |||
|35 | |||
|37 | |||
|- | |||
|Burmese bamboo | |||
|'']'' | |||
|95.1 | |||
| | |||
|32.1 | |||
|28.3 | |||
|- | |||
| | |||
|'']'' | |||
|air dry | |||
| | |||
|57 | |||
|51.77 | |||
|- | |||
|Indian timber bamboo | |||
|'']'' | |||
|73.6 | |||
| | |||
|40.7 | |||
|51.1 | |||
|- | |||
|Indian timber bamboo | |||
|'']'' | |||
|11.9 | |||
| | |||
|68 | |||
|66.7 | |||
|- | |||
|Indian timber bamboo | |||
|'']'' | |||
|8.6 | |||
|910 | |||
|79 | |||
|194 | |||
|- | |||
|dragon bamboo | |||
|'']'' | |||
|8 | |||
|740 | |||
|70 | |||
|193 | |||
|- | |||
|Hamilton's bamboo | |||
|'']'' | |||
|8.5 | |||
|590 | |||
|70 | |||
|89 | |||
|- | |||
|White bamboo | |||
|'']'' | |||
|102 | |||
| | |||
|40.5 | |||
|26.3 | |||
|- | |||
|String Bamboo | |||
|'']'' | |||
|54.3 | |||
| | |||
|24.1 | |||
|102 | |||
|- | |||
|String Bamboo | |||
|'']'' | |||
|15.1 | |||
| | |||
|37.95 | |||
|87.5 | |||
|- | |||
|Java Black Bamboo | |||
|'']'' | |||
|54 | |||
| | |||
|23.8 | |||
|92.3 | |||
|- | |||
|Java Black Bamboo | |||
|'']'' | |||
|15 | |||
| | |||
|35.7 | |||
|94.1 | |||
|- | |||
|Giant Atter | |||
|'']'' | |||
|72.3 | |||
| | |||
|26.4 | |||
|98 | |||
|- | |||
|Giant Atter | |||
|'']'' | |||
|14.4 | |||
| | |||
|31.95 | |||
|122.7 | |||
|- | |||
| | |||
|'']'' | |||
|8 | |||
|960 | |||
|71 | |||
|154 | |||
|- | |||
|American Narrow-Leaved Bamboo | |||
|'']'' | |||
| | |||
| | |||
|42 | |||
|53.5 | |||
|- | |||
|American Narrow-Leaved Bamboo | |||
|'']'' | |||
| | |||
| | |||
|63.6 | |||
|144.8 | |||
|- | |||
|American Narrow-Leaved Bamboo | |||
|'']'' | |||
| | |||
| | |||
|86.3 | |||
|46 | |||
|- | |||
|American Narrow-Leaved Bamboo | |||
|'']'' | |||
| | |||
| | |||
|77.5 | |||
|82 | |||
|- | |||
|American Narrow-Leaved Bamboo | |||
|'']'' | |||
|15 | |||
| | |||
|56 | |||
|87 | |||
|- | |||
|American Narrow-Leaved Bamboo | |||
|'']'' | |||
| | |||
| | |||
|63.3 | |||
| | |||
|- | |||
|American Narrow-Leaved Bamboo | |||
|'']'' | |||
| | |||
| | |||
|28 | |||
| | |||
|- | |||
|American Narrow-Leaved Bamboo | |||
|'']'' | |||
| | |||
| | |||
|56.2 | |||
| | |||
|- | |||
|American Narrow-Leaved Bamboo | |||
|'']'' | |||
| | |||
| | |||
|38 | |||
| | |||
|- | |||
|Berry Bamboo | |||
|'']'' | |||
|12.8 | |||
| | |||
|69.9 | |||
|57.6 | |||
|- | |||
|Japanese timber bamboo | |||
|'']'' | |||
| | |||
| | |||
|51 | |||
| | |||
|- | |||
|Japanese timber bamboo | |||
|'']'' | |||
|8 | |||
|730 | |||
|63 | |||
| | |||
|- | |||
|Japanese timber bamboo | |||
|'']'' | |||
|64 | |||
| | |||
|44 | |||
| | |||
|- | |||
|Japanese timber bamboo | |||
|'']'' | |||
|61 | |||
| | |||
|40 | |||
| | |||
|- | |||
|Japanese timber bamboo | |||
|'']'' | |||
|9 | |||
| | |||
|71 | |||
| | |||
|- | |||
|Japanese timber bamboo | |||
|'']'' | |||
|9 | |||
| | |||
|74 | |||
| | |||
|- | |||
|Japanese timber bamboo | |||
|'']'' | |||
|12 | |||
| | |||
|54 | |||
| | |||
|- | |||
|Tortoise shell bamboo | |||
|'']'' | |||
| | |||
| | |||
|44.6 | |||
| | |||
|- | |||
|Tortoise shell bamboo | |||
|'']'' | |||
|75 | |||
| | |||
|67 | |||
| | |||
|- | |||
|Tortoise shell bamboo | |||
|'']'' | |||
|15 | |||
| | |||
|71 | |||
| | |||
|- | |||
|Tortoise shell bamboo | |||
|'']'' | |||
|6 | |||
| | |||
|108 | |||
| | |||
|- | |||
|Tortoise shell bamboo | |||
|'']'' | |||
|0.2 | |||
| | |||
|147 | |||
| | |||
|- | |||
|Tortoise shell bamboo | |||
|'']'' | |||
|5 | |||
| | |||
|117 | |||
|51 | |||
|- | |||
|Tortoise shell bamboo | |||
|'']'' | |||
|30 | |||
| | |||
|44 | |||
|55 | |||
|- | |||
|Tortoise shell bamboo | |||
|'']'' | |||
|12.5 | |||
|603 | |||
|60.3 | |||
| | |||
|- | |||
|Tortoise shell bamboo | |||
|'']'' | |||
|10.3 | |||
|530 | |||
| | |||
|83 | |||
|- | |||
|Early Bamboo | |||
|'']'' | |||
|28.5 | |||
|827 | |||
|79.3 | |||
| | |||
|- | |||
|Oliveri | |||
|'']'' | |||
|53 | |||
| | |||
|46.9 | |||
|61.9 | |||
|- | |||
|Oliveri | |||
|'']'' | |||
|7.8 | |||
| | |||
|58 | |||
|90 | |||
|} | |||
==Hard versus soft== | |||
It is common to classify wood as either ] or ]. The wood from ] (e.g. pine) is called softwood, and the wood from ] (usually broad-leaved trees, e.g. oak) is called hardwood. These names are a bit misleading, as hardwoods are not necessarily hard, and softwoods are not necessarily soft. The well-known balsa (a hardwood) is actually softer than any commercial softwood. Conversely, some softwoods (e.g. ]) are harder than many hardwoods. | |||
There is a strong relationship between the properties of wood and the properties of the particular tree that yielded it, at least for certain species. For example, in loblolly pine, wind exposure and stem position greatly affect the hardness of wood, as well as compression wood content.<ref>{{cite book |title=Agriculture Handbook |date=1997 |publisher=U.S. Department of Agriculture |pages=2–6 |url=https://books.google.com/books?id=MeAstagRCJ4C&pg=SA2-PA6 |language=en |access-date=March 20, 2023 |archive-date=September 8, 2023 |archive-url=https://web.archive.org/web/20230908234052/https://books.google.com/books?id=MeAstagRCJ4C&pg=SA2-PA6 |url-status=live }}</ref> The density of wood varies with species. The density of a wood correlates with its strength (mechanical properties). For example, ] is a medium-dense hardwood that is excellent for fine furniture crafting, whereas ] is light, making it useful for ] building. One of the densest woods is ]. | |||
==Chemistry== | |||
], which makes up about 25% of wood dry matter and is responsible for many of its properties.]] | |||
The chemical composition of wood varies from species to species, but is approximately 50% carbon, 42% oxygen, 6% hydrogen, 1% nitrogen, and 1% other elements (mainly ], ], ], ], ], and ]) by weight.<ref>{{cite book|title=Mémotech Bois et Matériaux Associés|date=1996|publisher=Éditions Casteilla|location=Paris|isbn=978-2-7135-1645-0|page=22|author= Jean-Pierre Barette|author2= Claude Hazard et Jérôme Mayer}}</ref> Wood also contains ], ], ], ], and other elements in small quantity. | |||
Aside from water, wood has three main components. ], a crystalline polymer derived from glucose, constitutes about 41–43%. Next in abundance is ], which is around 20% in deciduous trees but near 30% in conifers. It is mainly ] that are linked in an irregular manner, in contrast to the cellulose. ] is the third component at around 27% in coniferous wood vs. 23% in deciduous trees. Lignin confers the hydrophobic properties reflecting the fact that it is based on ]s. These three components are interwoven, and direct covalent linkages exist between the lignin and the hemicellulose. A major focus of the paper industry is the separation of the lignin from the cellulose, from which paper is made. | |||
In chemical terms, the difference between hardwood and softwood is reflected in the composition of the constituent ]. Hardwood lignin is primarily derived from ] and ]. Softwood lignin is mainly derived from coniferyl alcohol.<ref name="Boerjan-2003">{{cite journal| author = W. Boerjan| author2 = J. Ralph| author3 = M. Baucher|date=June 2003| title = Lignin biosynthesis| journal = Annu. Rev. Plant Biol.| volume = 54| issue = 1| pages = 519–549| doi = 10.1146/annurev.arplant.54.031902.134938| pmid = 14503002}}</ref> | |||
===Extractives=== | |||
Aside from the structural ]s, i.e. ], ] and ] (]), wood contains a large variety of non-structural constituents, composed of low ] ]s, called ''extractives''. These compounds are present in the ] and can be extracted from the wood using different neutral ]s, such as ].<ref name="Ek-2009">{{cite book |last1=Ek |first1=Monica |last2=Gellerstedt |first2=Göran |last3=Henriksson |first3=Gunnar |title=Pulp and Paper Chemistry and Technology. Volume 1, Wood Chemistry and Wood Biotechnology |date=2009 |publisher=Walter de Gruyter |location=Berlin |isbn=978-3-11-021339-3 |chapter=Chapter 7: Wood extractives}}</ref> Analogous content is present in the so-called ''exudate'' produced by trees in response to mechanical damage or after being attacked by ]s or ].<ref name="Sjöström-2013">{{cite book |last1=Sjöström |first1=Eero |title=Wood Chemistry: Fundamentals and Applications |publisher=Elsevier Science |location=San Diego |isbn=978-0-08-092589-9 |edition=Second |chapter=Chapter 5: Extractives|date=October 22, 2013 }}</ref> Unlike the structural constituents, the composition of extractives varies over wide ranges and depends on many factors.<ref>{{cite book |last1=Ansell |first1=Martin P. |title=Woodhead Publishing Series in Composites Science and Engineering: Number 54. Wood Composites |date=2015 |publisher=Woodhead Publishing |location=Cambridge, UK |isbn=978-1-78242-454-3 |chapter=Chapter 11: Preservation, Protection and Modification of Wood Composites}}</ref> The amount and composition of extractives differs between tree species, various parts of the same tree, and depends on genetic factors and growth conditions, such as climate and geography.<ref name="Ek-2009" /> For example, slower growing trees and higher parts of trees have higher content of extractives. Generally, the ] is richer in extractives than the ]. Their concentration increases from the ] to the ]. ]s and ]es also contain extractives. Although extractives represent a small fraction of the wood content, usually less than 10%, they are extraordinarily diverse and thus characterize the chemistry of the wood species.<ref name="Hon-2001">{{cite book |last1=Hon |first1=David N.-S. |last2=Shiraishi |first2=Nubuo |title=Wood and Cellulosic Chemistry |date=2001 |publisher=Marcel Dekker |location=New York |isbn=0-8247-0024-4 |edition=2nd, rev. and expanded |chapter=Chapter 6: Chemistry of Extractives}}</ref> Most extractives are secondary metabolites and some of them serve as precursors to other chemicals. Wood extractives display different activities, some of them are produced in response to wounds, and some of them participate in natural defense against insects and fungi.<ref>{{cite book |last1=Rowell |first1=Roger M. |title=Handbook of Wood Chemistry and Wood Composites |date=2013 |publisher=Taylor & Francis |location=Boca Raton |isbn=9781439853801 |edition=2nd |chapter=Chater 3: Cell Wall Chemistry}}</ref> | |||
] refinery in ], Finland]] | |||
These compounds contribute to various physical and chemical properties of the wood, such as wood color, fragnance, durability, acoustic properties, ], adhesion, and drying.<ref name="Hon-2001" /> Considering these impacts, wood extractives also affect the properties of ] and paper, and importantly cause many problems in ]. Some extractives are surface-active substances and unavoidably affect the surface properties of paper, such as water adsorption, friction and strength.<ref name="Ek-2009" /> ] extractives often give rise to sticky deposits during ] and may leave spots on paper. Extractives also account for paper smell, which is important when making ]. | |||
Most wood extractives are ] and only a little part is water-soluble.<ref name="Sjöström-2013" /> The lipophilic portion of extractives, which is collectively referred as wood ], contains ]s and ]s, ]s and steryl esters, ]s, ]s, ]s, and ]es.<ref>{{cite book |last = Mimms |first = Agneta |author2=Michael J. Kuckurek |author3=Jef A. Pyiatte |author4=Elizabeth E. Wright |title = Kraft Pulping. A Compilation of Notes |publisher = TAPPI Press |date = 1993 |pages = 6–7 |isbn = 978-0-89852-322-5 }}</ref> The heating of resin, i.e. ], vaporizes the ] terpenes and leaves the solid component – ]. The concentrated liquid of volatile compounds extracted during ] is called ]. Distillation of ] obtained from many ] provides ] and ].<ref>{{cite book |doi=10.1002/14356007.a23_073 |chapter=Resins, Natural |title=Ullmann's Encyclopedia of Industrial Chemistry |date=2000 |last1=Fiebach |first1=Klemens |last2=Grimm |first2=Dieter |isbn=978-3-527-30673-2}}</ref> | |||
Most extractives can be categorized into three groups: ]s, ]s and ].<ref name="Ek-2009" /> The latter are more water-soluble and usually are absent in the resin. | |||
*]s include fatty acids, ]s and their esters with ], fatty alcohols (waxes) and sterols (steryl esters). ]s, such as ]s, are also present in the wood. ] is a polyester, made of suberin acids and glycerol, mainly found in ]s. Fats serve as a source of energy for the wood cells.<ref name="Sjöström-2013" /> The most common wood sterol is ], and less commonly ], citrostadienol, ] or ].<ref name="Ek-2009" /> | |||
*The main ]s occurring in the softwood include ], ] and ]s.<ref name="Sjöström-2013" /> Meanwhile, the terpene composition of the hardwood is considerably different, consisting of ]s, ]s and other higher terpenes. Examples of mono-, di- and sesquiterpenes are ] and ]s, ], ], ], ]s, α- and β-]s, α-muurolene, ], ] and ]s, α- and β-]s, juniperol, ], ''cis''-abienol, ], pinifolic acid, nootkatin, chanootin, ], geranyl-linalool, β-epimanool, manoyloxide, pimaral and pimarol. Resin acids are usually ] ]s, examples of which are ], sandaracopimaric acid, ], ], ], palustric acid, neoabietic acid and dehydroabietic acid. ] resin acids are also found, such as lambertianic acid, communic acid, mercusic acid and secodehydroabietic acid. ], ] and ] are ]s purified from hardwood. Examples of wood polyterpenes are ] (''cis''-polypren), ] (''trans''-polypren), gutta-balatá (''trans''-polypren) and betulaprenols (] polyterpenoids).<ref name="Ek-2009" /><ref name="Sjöström-2013" /> The mono- and sesquiterpenes of the softwood are responsible for the typical smell of ] forest.<ref name="Ek-2009" /> Many monoterpenoids, such as ], are used in the preparation of ]s and ].<ref name="Sjöström-2013" /> ]s, such as ] and other ]s, are present in ]-resistant trees and display ] and ] properties. Tropolones strongly bind metal ions and can cause digester ] in the process ]. Owing to their ] and ] properties, especially thujaplicins are used in physiology experiments.<ref>{{cite book |title=Cell physiology sourcebook: essentials of membrane biophysics |location=London, UK |isbn=978-0-12-387738-3 |edition=Fourth |chapter=Chapter 4: Ionophores in Planar Lipid Bilayers |chapter-url=https://www.sciencedirect.com/science/article/pii/B9780123877383000044 |last1=Sperelakis |first1=Nicholas |last2=Sperelakis |first2=Nick |date=January 11, 2012 |access-date=September 27, 2020 |archive-date=June 28, 2020 |archive-url=https://web.archive.org/web/20200628201941/https://www.sciencedirect.com/science/article/pii/B9780123877383000044 |url-status=live }}</ref> Different other ''in-vitro'' biological activities of thujaplicins have been studied, such as insecticidal, anti-browning, anti-viral, anti-bacterial, anti-fungal, anti-proliferative and anti-oxidant.<ref>{{cite journal |last1=Saniewski |first1=Marian |last2=Horbowicz |first2=Marcin |last3=Kanlayanarat |first3=Sirichai |title=The Biological Activities of Troponoids and Their Use in Agriculture A Review |journal=Journal of Horticultural Research |date=10 September 2014 |volume=22 |issue=1 |pages=5–19 |doi=10.2478/johr-2014-0001|s2cid=33834249 |doi-access=free }}</ref><ref>{{cite journal |last1=Bentley |first1=Ronald |title=A fresh look at natural tropolonoids |journal=Nat. Prod. Rep. |date=2008 |volume=25 |issue=1 |pages=118–138 |doi=10.1039/b711474e|pmid=18250899 }}</ref> | |||
*] are especially found in the hardwood and the bark.<ref name="Sjöström-2013" /> The most well-known wood phenolic constituents are ] (e.g. ]), ] (e.g. ], conidendrin, ], ]), norlignans (e.g. ], puerosides A and B, hydroxysugiresinol, sequirin-C), ]s (e.g. ], ]), ]s (e.g. ], ], ], ]). Most of the phenolic compounds have fungicidal properties and protect the wood from ].<ref name="Sjöström-2013" /> Together with the neolignans the phenolic compounds influence on the color of the wood. Resin acids and phenolic compounds are the main toxic contaminants present in the untreated ]s from ].<ref name="Ek-2009" /> ] compounds are one of the most abundant biomolecules produced by plants, such as ]s and ]s. Tannins are used in ] industry and have shown to exhibit different biological activities.<ref name="Hon-2001" /> ]s are very diverse, widely distributed in the ] kingdom and have numerous biological activities and roles.<ref name="Sjöström-2013" /> | |||
==Uses== | ==Uses== | ||
] | |||
] | |||
=== Production === | |||
{{Main|Forestry}} | |||
Global production of roundwood rose from 3.5 billion m''³'' in 2000 to 4 billion m''³'' in 2021. In 2021, wood fuel was the main product with a 49 percent share of the total (2 billion m''³''), followed by coniferous industrial roundwood with 30 percent (1.2 billion m''³'') and non-coniferous industrial roundwood with 21 percent (0.9 billion m''³''). Asia and the Americas are the two main producing regions, accounting for 29 and 28 percent of the total roundwood production, respectively; Africa and Europe have similar shares of 20–21 percent, while Oceania produces the remaining 2 percent.<ref name="FAO-2023">{{Cite book |url=http://www.fao.org/documents/card/en/c/cc8166en |title=World Food and Agriculture – Statistical Yearbook 2023 |date=2023-11-29 |publisher=FAO |isbn=978-92-5-138262-2 |language=en |doi=10.4060/cc8166en}}</ref> | |||
===Fuel=== | ===Fuel=== | ||
{{Main|Wood fuel}} | {{Main|Wood fuel}} | ||
Wood has a long history of being used as fuel, which continues to this day, mostly in rural areas of the world. Hardwood is preferred over softwood because it creates less smoke and burns longer. Adding a woodstove or fireplace to a home is often felt to add ambiance and warmth. |
Wood has a long history of being used as fuel,<ref>{{Cite book|url=https://books.google.com/books?id=jFvrF4DaZcgC&q=%C2%A0Wood+has+a+long+history+of+being+used+as+fuel&pg=PA261|title=Alternative Fuels and the Environment|last=Sterrett|first=Frances S.|date=1994-10-12|publisher=CRC Press|isbn=978-0-87371-978-0|language=en|df=mdy-all|access-date=October 6, 2020|archive-date=December 30, 2023|archive-url=https://web.archive.org/web/20231230131945/https://books.google.com/books?id=jFvrF4DaZcgC&q=%C2%A0Wood+has+a+long+history+of+being+used+as+fuel&pg=PA261#v=snippet&q=%C2%A0Wood%20has%20a%20long%20history%20of%20being%20used%20as%20fuel&f=false|url-status=live}}</ref> which continues to this day, mostly in rural areas of the world. Hardwood is preferred over softwood because it creates less smoke and burns longer. Adding a woodstove or fireplace to a home is often felt to add ambiance and warmth. | ||
===Pulpwood=== | |||
Pulpwood is wood that is raised specifically for use in making paper. | |||
===Construction=== | ===Construction=== | ||
].]] | |||
], ], ], ] built in ] is made of and decorated in wood.<ref>“”,''DykerHeightsCivicAssociation.com''</ref>]] | |||
Wood has been an important construction material since humans began building shelters, ]s and ]s. Nearly all boats were made out of wood until the late 19th century, and wood remains in common use today in boat construction. | |||
], ], ], New York built in 1899 is made of and decorated in wood.<ref>" {{webarchive|url=https://web.archive.org/web/20081216233832/http://www.dykerheightscivicassociation.com/saittareport.pdf |date=December 16, 2008 }}",''DykerHeightsCivicAssociation.com''</ref>]] | |||
Wood to be used for construction work is commonly known as '']'' in ]. Elsewhere, ''lumber'' usually refers to felled trees, and the word for sawn planks ready for use is ''timber''. | |||
] | |||
Wood has been an important construction material since humans began building shelters, houses and boats. Nearly all boats were made out of wood until the late 19th century, and wood remains in common use today in boat construction. ] in particular was used for this purpose as it resisted decay as long as it was kept wet (it also served for water pipe before the advent of more modern plumbing). | |||
Wood to be used for construction work is commonly known as '']'' in North America. Elsewhere, ''lumber'' usually refers to felled trees, and the word for sawn planks ready for use is ''timber''.<ref>{{Cite book|url=https://books.google.com/books?id=jSiRAAAAQBAJ&q=%C2%A0Wood+to+be+used+for+construction+work+is+commonly+known+as+lumber+in+North+America&pg=SA7-PA15|title=Materials for Interior Environments|last=Binggeli|first=Corky|year=2013|publisher=John Wiley & Sons|isbn=978-1-118-42160-4|language=en|df=mdy-all|access-date=October 6, 2020|archive-date=December 30, 2023|archive-url=https://web.archive.org/web/20231230132013/https://books.google.com/books?id=jSiRAAAAQBAJ&q=%C2%A0Wood+to+be+used+for+construction+work+is+commonly+known+as+lumber+in+North+America&pg=SA7-PA15#v=snippet&q=%C2%A0Wood%20to%20be%20used%20for%20construction%20work%20is%20commonly%20known%20as%20lumber%20in%20North%20America&f=false|url-status=live}}</ref> In Medieval Europe ] was the wood of choice for all wood construction, including beams, walls, doors, and floors. Today a wider variety of woods is used: solid wood doors are often made from ], small-knotted ], and ]. | |||
], Russia are among a handful of ]s built entirely of wood, without metal joints. See ] for more details.]] | |||
New domestic housing in many parts of the world today is commonly made from timber-framed construction. ] products are becoming a bigger part of the construction industry. They may be used in both residential and commercial buildings as structural and aesthetic materials. | New domestic housing in many parts of the world today is commonly made from timber-framed construction. ] products are becoming a bigger part of the construction industry. They may be used in both residential and commercial buildings as structural and aesthetic materials. | ||
In buildings made of other materials, wood will still be found as a supporting material, especially in |
In buildings made of other materials, wood will still be found as a supporting material, especially in roof construction, in interior doors and their frames, and as exterior cladding. | ||
Wood is also commonly used as shuttering material to form the |
Wood is also commonly used as shuttering material to form the mold into which concrete is poured during ] construction. | ||
====Flooring==== | |||
{{clear}} | |||
].]] | |||
{{Main |Wood flooring}}A solid wood floor is a floor laid with planks or battens created from a single piece of timber, usually a hardwood. Since wood is hydroscopic (it acquires and loses moisture from the ambient conditions around it) this potential instability effectively limits the length and width of the boards. | |||
Solid hardwood flooring is usually cheaper than engineered timbers and damaged areas can be sanded down and refinished repeatedly, the number of times being limited only by the thickness of wood above the tongue. | |||
==== Engineered wood ==== | |||
Wood used in construction includes products such as ] (glulam), ] (LVL), ] and ]s. On the one hand these allow the use of smaller pieces, and on the other hand allow bigger spans. They may also be selected for specific projects such as public swimming pools or ice rinks where the wood will not deteriorate in the presence of certain chemicals. These engineered wood products prove to be more environmentally friendly, and sometimes cheaper, than building materials such as steel or concrete. | |||
Solid hardwood floors were originally used for structural purposes, being installed perpendicular to the wooden support beams of a building (the joists or bearers) and solid construction timber is still often used for sports floors as well as most traditional wood blocks, ]s and ]. | |||
Wood unsuitable for construction in its native form may be broken down mechanically (into fibers or chips) or chemically (into cellulose) and used as a raw material for other building materials such as ], ], ], ] (MDF), ] (OSB). Such wood derivatives are widely used: wood fibers are an important component of most ], and cellulose is used as a component of some ]s. Wood derivatives can also be used for kinds of flooring, for example ]. | |||
==== |
====Engineered products==== | ||
{{main |Engineered wood}} | |||
Further developments include new ] glue applications, recyclable food packaging, rubber tire replacement applications, anti-bacterial medical agents, and high strength fabrics or composites.<ref>http://www.forintek.ca/public/pdf/annual%20report/AR_2007_2008/AR_ENG_2007.pdf</ref> | |||
As scientists and engineers further learn and develop new techniques to extract various components from wood, or alternatively to modify wood, for example by adding components to wood, new more advanced products will appear on the marketplace. | |||
Engineered wood products, glued building products "engineered" for application-specific performance requirements, are often used in construction and industrial applications. Glued engineered wood products are manufactured by bonding together wood strands, veneers, lumber or other forms of wood fiber with glue to form a larger, more efficient composite structural unit.<ref name="apawood">{{cite web|url=http://www.apawood.org/pdfs/download_pdf.cfm?PDFFilename=managed/E30.pdf|title=APA – The Engineered Wood Association|work=apawood.org|url-status=live|archive-url=https://web.archive.org/web/20060627045932/http://www.apawood.org/pdfs/download_pdf.cfm?PDFFilename=managed%2FE30.pdf|archive-date=June 27, 2006|df=mdy-all}}</ref> | |||
=== Furniture and utensils === | |||
Wood has always been used extensively for furniture, including ] and ]s. Also for tool handles and cutlery, such as ], ]s, and other utensils, like the ]. | |||
These products include ] (glulam), wood structural panels (including ], ] and composite panels), ] (LVL) and other structural composite lumber (SCL) products, ], and I-joists.<ref name="apawood" /> Approximately 100 million cubic meters of wood was consumed for this purpose in 1991.<ref name="Horst-2005"/> The trends suggest that particle board and fiber board will overtake plywood. | |||
===In the arts=== | |||
]s can use wood to create delicate ]s.]] | |||
] or ].]] | |||
{{Main|Wood as a medium}} | |||
Wood has long been used as an ]. It has been used to make ]s and ] for millennia. Examples include the ]s carved by North American indigenous people from conifer trunks, often Western Red Cedar ('']''), and the Millennium clock tower <ref>http://freespace.virgin.net/sharmanka.kinetic/clocktower/</ref>, now housed in the ]<ref>http://www.nms.ac.uk/nationalmuseumhomepage.aspx</ref> in ]. | |||
Wood unsuitable for construction in its native form may be broken down mechanically (into fibers or chips) or chemically (into cellulose) and used as a raw material for other building materials, such as engineered wood, as well as ], ], and ] (MDF). Such wood derivatives are widely used: wood fibers are an important component of most paper, and cellulose is used as a component of some ]. Wood derivatives can be used for kinds of flooring, for example ]. | |||
It is also used in ] ], and for ]. | |||
===Furniture and utensils=== | |||
Certain types of ]s, such as those of the ], the ], the ] and ], the ], and the ], are made mostly or entirely of wood. The choice of wood may make a significant difference to the tone and resonant qualities of the instrument, and ]s have widely differing properties, ranging from the hard and dense ] (used for the bodies of clarinets) to the light but resonant European spruce ('']'') (traditionally used for the soundboards of violins). The most valuable tonewoods, such as the ripple sycamore ('']''), used for the backs of violins, combine acoustic properties with decorative color and grain which enhance the appearance of the finished instrument. | |||
Wood has always been used extensively for ], such as ] and beds. It is also used for tool handles and cutlery, such as ], ]s, and other utensils, like the ] and ]. | |||
===Other=== | |||
Despite their collective name, not all ]s are made entirely of wood. The ] used to play them, however, are usually made from '']'', a type of ] ] plant. | |||
Further developments include new ] glue applications, recyclable food packaging, rubber tire replacement applications, anti-bacterial medical agents, and high strength fabrics or composites.<ref>{{cite web|url=http://www.forintek.ca/public/pdf/annual%20report/AR_2007_2008/AR_ENG_2007.pdf|title=FPInnovations|work=forintek.ca|url-status=dead|archive-url=https://web.archive.org/web/20090319100903/http://www.forintek.ca/public/pdf/annual%20report/AR_2007_2008/AR_ENG_2007.pdf|archive-date=March 19, 2009|df=mdy-all}}</ref> | |||
As scientists and engineers further learn and develop new techniques to extract various components from wood, or alternatively to modify wood, for example by adding components to wood, new more advanced products will appear on the marketplace. Moisture content electronic monitoring can also enhance next generation wood protection.<ref>"System for remotely monitoring moisture content on wooden elements" I Arakistain, O Munne EP Patent EPO1382108.0</ref> | |||
===Art=== | |||
{{clear}} | |||
]'', ]]] | |||
Wood has long been used as an ]. It has been used to make sculptures and ] for millennia. Examples include the ]s carved by North American indigenous people from conifer trunks, often Western Red Cedar ('']''). | |||
Other uses of wood in the arts include: | |||
* ] ] and ] | |||
* Wood can be a surface to paint on, such as in ] | |||
* Many ]s are made mostly or entirely of wood | |||
===Sports and recreational equipment=== | ===Sports and recreational equipment=== | ||
Many types of ] are made of wood, or were constructed of wood in the past. |
Many types of ] are made of wood, or were constructed of wood in the past. For example, ]s are typically made of ]. The ]s which are legal for use in ] are frequently made of ] or ], and in recent years have been constructed from ] even though that wood is somewhat more fragile. ] courts have been traditionally made out of ]. | ||
Many other types of sports and recreation equipment, such as ]s, ]s, lacrosse |
Many other types of sports and recreation equipment, such as ]s, ]s, ]s and ], were commonly made of wood in the past, but have since been replaced with more modern materials such as aluminium, ] or ]s such as ] and ]. One noteworthy example of this trend is the family of ] commonly known as the '']'', the heads of which were traditionally made of ] wood in the early days of the game of golf, but are now generally made of metal or (especially in the case of ]) carbon-fiber composites. | ||
==Bacterial degradation== | |||
===Medicine=== | |||
Little is known about the bacteria that degrade cellulose. ] in '']'' may play a role in the degradation of sunken wood. '']'', '']'', '']'', '']'', and '']'' have been detected in wood submerged for over a year.<ref>{{cite journal|title=How Deep-Sea Wood Falls Sustain Chemosynthetic Life|author1=Christina Bienhold|author2=Petra Pop Ristova|author3=Frank Wenzhöfer|author4=Thorsten Dittmar|author5=Antje Boetius|journal=PLOS ONE|volume = 8|issue=1|pages=e53590|date=January 2, 2013|df=mdy-all|doi=10.1371/journal.pone.0053590|pmid=23301092|pmc=3534711|bibcode = 2013PLoSO...853590B|doi-access=free}}</ref> | |||
In January 2010 Italian scientists announced that wood could be harnessed to become a ]. It is likely to take at least five years until this technique will be applied for humans.<ref>{{cite news| url=http://news.bbc.co.uk/1/hi/health/8438209.stm | work=BBC News | title=Scientists make bones from wood | date=2010-01-03}}</ref> | |||
<!-- | <!-- | ||
DO ''not'' ADD A "Popular culture" SECTION HERE. There has been extensive discussion about why this is inappropriate on the article's talk page. Adding a "Pop culture" section based on the xkcd comic will be viewed as vandalism--it isn't clever or funny. Any such addition will be subsequently removed, and you may be banned from editing further.--> | |||
DO NOT ADD A "Popular culture" SECTION HERE. | |||
There has been extensive discussion about why this is inappropriate on the article's talk page. Adding a "Pop culture" section based on the xkcd comic will be viewed as vandalism--it isn't clever or funny. Any such addition will be subsequently removed, and you may be banned from editing further. | |||
--> | |||
==See also== | ==See also== | ||
{{ |
{{Portal|Trees}} | ||
{{div col|colwidth=20em}} | |||
* ] | |||
* ] | |||
* ] | |||
* ] | * ] | ||
* ] | * ] | ||
* ] | |||
* ] | |||
* ] | |||
* ] | * ] | ||
* ] | * ] | ||
* ] | * ] | ||
* ] | |||
* ] | |||
* ] | |||
* ] | |||
* ] | |||
* ] | |||
* ] | * ] | ||
* ] | |||
{{multicol-break}} | |||
* ] | * ] | ||
* ] | |||
* ] | |||
* ] | |||
* ] | |||
* ] | * ] | ||
* ] | * ] | ||
* ] | |||
* ] | |||
* ] | |||
* ] | |||
* ] | |||
* ] | |||
* ] | |||
* ] | * ] | ||
* ] | |||
{{multicol-break}} | |||
* ] | |||
* ] | |||
* ] | |||
* ] | * ] | ||
* ] | * ] | ||
* ] | |||
* ] | * ] | ||
* ] | * ] | ||
* ] | * ] | ||
* ] | |||
{{multicol-break}} | |||
* ] | * ] | ||
* ] | |||
* ] | * ] | ||
* ] | |||
* ] | |||
* ] | |||
* ] | * ] | ||
* ] | * ] | ||
* ] | |||
* ] | * ] | ||
* ] | * ] | ||
{{multicol-break}} | |||
* ] | * ] | ||
* ] | * ] | ||
* ] | * ] | ||
* '']'' | |||
{{multicol-end}} | |||
{{div col end}} | |||
== |
==Sources== | ||
{{Free-content attribution | |||
| title = World Food and Agriculture – Statistical Yearbook 2023 | |||
| author = | |||
| publisher = FAO | |||
| documentURL = https://www.fao.org/documents/card/en?details=cc8166en | |||
| license statement URL = https://commons.wikimedia.org/File:World_Food_and_Agriculture_-_Statistical_Yearbook_2023.pdf <!-- Also in the document itself --> | |||
| license = CC BY-SA IGO 3.0 | |||
}} | |||
==References== | |||
{{reflist|2}} | |||
{{reflist|30em}} | |||
* {{cite book |author-link = R. Bruce Hoadley |last = Hoadley |first = R. Bruce |date = 2000 |title = Understanding Wood: A Craftsman's Guide to Wood Technology |publisher = ] |isbn = 978-1-56158-358-4 }} | |||
== References == | |||
{{Commons category}} | |||
{{Wiktionary}} | |||
{{refbegin}} | |||
* {{ cite book | authorlink = R. Bruce Hoadley | last = Hoadley | first = R. Bruce | date = 2000 | title = Understanding Wood: A Craftsman’s Guide to Wood Technology | publisher = ] | isbn = 1-56158-358-8 }} | |||
* Shigo, Alex. (1986) ''A New Tree Biology Dictionary''. Shigo and Trees, Associates. ISBN 0-943563-12-7 | |||
* | |||
* | |||
{{refend}} | |||
==External links== | |||
{{commons category}} | |||
* (archived 27 May 2016) | |||
* ({{Webarchive|url=https://web.archive.org/web/20150407062512/http://www.thewoodexplorer.com/ |date=April 7, 2015 }}) | |||
* (archived 14 April 2011) | |||
{{Botany}} | {{Botany}} | ||
{{Forestry}} | |||
{{Wood products}} | |||
{{Woodworking}} | |||
{{Natural resources}} | |||
{{Tannin source}} | |||
{{Sculptures}} | |||
{{Authority control}} | |||
{{Portal bar|Arthropods|Ecology|Engineering|Environment|Fungi|Islands|Painting|Trains|Trees}} | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | ] | ||
] | ] | ||
] | ] | ||
] | ] | ||
] | ] | ||
] | ] | ||
] | ] | ||
] | ] | ||
] | ] | ||
] | ] | ||
] | |||
] | |||
{{Link FA|hu}} | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] | |||
] |
Latest revision as of 14:50, 13 November 2024
Fibrous material from trees or other plantsFor a small forest, see Woodland. For wood as a commodity, see Timber. For other uses, see Wood (disambiguation) and Wooden (disambiguation).
Wood samples Pine Spruce Larch Juniper Aspen Hornbeam Birch Alder Beech Oak Elm Cherry Pear Maple Linden Ash |
Wood is a structural tissue/material found as xylem in the stems and roots of trees and other woody plants. It is an organic material – a natural composite of cellulosic fibers that are strong in tension and embedded in a matrix of lignin that resists compression. Wood is sometimes defined as only the secondary xylem in the stems of trees, or more broadly to include the same type of tissue elsewhere, such as in the roots of trees or shrubs. In a living tree, it performs a mechanical-support function, enabling woody plants to grow large or to stand up by themselves. It also conveys water and nutrients among the leaves, other growing tissues, and the roots. Wood may also refer to other plant materials with comparable properties, and to material engineered from wood, woodchips, or fibers.
Wood has been used for thousands of years for fuel, as a construction material, for making tools and weapons, furniture and paper. More recently it emerged as a feedstock for the production of purified cellulose and its derivatives, such as cellophane and cellulose acetate.
As of 2020, the growing stock of forests worldwide was about 557 billion cubic meters. As an abundant, carbon-neutral renewable resource, woody materials have been of intense interest as a source of renewable energy. In 2008, approximately 3.97 billion cubic meters of wood were harvested. Dominant uses were for furniture and building construction.
Wood is scientifically studied and researched through the discipline of wood science, which was initiated since the beginning of the 20th century.
History
A 2011 discovery in the Canadian province of New Brunswick yielded the earliest known plants to have grown wood, approximately 395 to 400 million years ago.
Wood can be dated by carbon dating and in some species by dendrochronology to determine when a wooden object was created.
People have used wood for thousands of years for many purposes, including as a fuel or as a construction material for making houses, tools, weapons, furniture, packaging, artworks, and paper. Known constructions using wood date back ten thousand years. Buildings like the longhouses in Neolithic Europe were made primarily of wood.
Recent use of wood has been enhanced by the addition of steel and bronze into construction.
The year-to-year variation in tree-ring widths and isotopic abundances gives clues to the prevailing climate at the time a tree was cut.
Physical properties
Growth rings
See also: Dendrochronology § Growth ringsWood, in the strict sense, is yielded by trees, which increase in diameter by the formation, between the existing wood and the inner bark, of new woody layers which envelop the entire stem, living branches, and roots. This process is known as secondary growth; it is the result of cell division in the vascular cambium, a lateral meristem, and subsequent expansion of the new cells. These cells then go on to form thickened secondary cell walls, composed mainly of cellulose, hemicellulose and lignin.
Where the differences between the seasons are distinct, e.g. New Zealand, growth can occur in a discrete annual or seasonal pattern, leading to growth rings; these can usually be most clearly seen on the end of a log, but are also visible on the other surfaces. If the distinctiveness between seasons is annual (as is the case in equatorial regions, e.g. Singapore), these growth rings are referred to as annual rings. Where there is little seasonal difference growth rings are likely to be indistinct or absent. If the bark of the tree has been removed in a particular area, the rings will likely be deformed as the plant overgrows the scar.
If there are differences within a growth ring, then the part of a growth ring nearest the center of the tree, and formed early in the growing season when growth is rapid, is usually composed of wider elements. It is usually lighter in color than that near the outer portion of the ring, and is known as earlywood or springwood. The outer portion formed later in the season is then known as the latewood or summerwood. There are major differences, depending on the kind of wood. If a tree grows all its life in the open and the conditions of soil and site remain unchanged, it will make its most rapid growth in youth, and gradually decline. The annual rings of growth are for many years quite wide, but later they become narrower and narrower. Since each succeeding ring is laid down on the outside of the wood previously formed, it follows that unless a tree materially increases its production of wood from year to year, the rings must necessarily become thinner as the trunk gets wider. As a tree reaches maturity its crown becomes more open and the annual wood production is lessened, thereby reducing still more the width of the growth rings. In the case of forest-grown trees so much depends upon the competition of the trees in their struggle for light and nourishment that periods of rapid and slow growth may alternate. Some trees, such as southern oaks, maintain the same width of ring for hundreds of years. On the whole, as a tree gets larger in diameter the width of the growth rings decreases.
Knots
As a tree grows, lower branches often die, and their bases may become overgrown and enclosed by subsequent layers of trunk wood, forming a type of imperfection known as a knot. The dead branch may not be attached to the trunk wood except at its base and can drop out after the tree has been sawn into boards. Knots affect the technical properties of the wood, usually reducing tension strength, but may be exploited for visual effect. In a longitudinally sawn plank, a knot will appear as a roughly circular "solid" (usually darker) piece of wood around which the grain of the rest of the wood "flows" (parts and rejoins). Within a knot, the direction of the wood (grain direction) is up to 90 degrees different from the grain direction of the regular wood.
In the tree a knot is either the base of a side branch or a dormant bud. A knot (when the base of a side branch) is conical in shape (hence the roughly circular cross-section) with the inner tip at the point in stem diameter at which the plant's vascular cambium was located when the branch formed as a bud.
In grading lumber and structural timber, knots are classified according to their form, size, soundness, and the firmness with which they are held in place. This firmness is affected by, among other factors, the length of time for which the branch was dead while the attaching stem continued to grow.
Knots materially affect cracking and warping, ease in working, and cleavability of timber. They are defects which weaken timber and lower its value for structural purposes where strength is an important consideration. The weakening effect is much more serious when timber is subjected to forces perpendicular to the grain and/or tension than when under load along the grain and/or compression. The extent to which knots affect the strength of a beam depends upon their position, size, number, and condition. A knot on the upper side is compressed, while one on the lower side is subjected to tension. If there is a season check in the knot, as is often the case, it will offer little resistance to this tensile stress. Small knots may be located along the neutral plane of a beam and increase the strength by preventing longitudinal shearing. Knots in a board or plank are least injurious when they extend through it at right angles to its broadest surface. Knots which occur near the ends of a beam do not weaken it. Sound knots which occur in the central portion one-fourth the height of the beam from either edge are not serious defects.
— Samuel J. Record, The Mechanical Properties of Wood
Knots do not necessarily influence the stiffness of structural timber; this will depend on the size and location. Stiffness and elastic strength are more dependent upon the sound wood than upon localized defects. The breaking strength is very susceptible to defects. Sound knots do not weaken wood when subject to compression parallel to the grain.
In some decorative applications, wood with knots may be desirable to add visual interest. In applications where wood is painted, such as skirting boards, fascia boards, door frames and furniture, resins present in the timber may continue to 'bleed' through to the surface of a knot for months or even years after manufacture and show as a yellow or brownish stain. A knot primer paint or solution (knotting), correctly applied during preparation, may do much to reduce this problem but it is difficult to control completely, especially when using mass-produced kiln-dried timber stocks.
Heartwood and sapwood
"Heartwood" redirects here. For other uses, see Heartwood (disambiguation). "Sapwood" redirects here. For the missile also called "SS-6 Sapwood", see R7 Semyorka. See also: Trunk (botany)Heartwood (or duramen) is wood that as a result of a naturally occurring chemical transformation has become more resistant to decay. Heartwood formation is a genetically programmed process that occurs spontaneously. Some uncertainty exists as to whether the wood dies during heartwood formation, as it can still chemically react to decay organisms, but only once.
The term heartwood derives solely from its position and not from any vital importance to the tree. This is evidenced by the fact that a tree can thrive with its heart completely decayed. Some species begin to form heartwood very early in life, so having only a thin layer of live sapwood, while in others the change comes slowly. Thin sapwood is characteristic of such species as chestnut, black locust, mulberry, osage-orange, and sassafras, while in maple, ash, hickory, hackberry, beech, and pine, thick sapwood is the rule. Some others never form heartwood.
Heartwood is often visually distinct from the living sapwood and can be distinguished in a cross-section where the boundary will tend to follow the growth rings. For example, it is sometimes much darker. Other processes such as decay or insect invasion can also discolor wood, even in woody plants that do not form heartwood, which may lead to confusion.
Sapwood (or alburnum) is the younger, outermost wood; in the growing tree it is living wood, and its principal functions are to conduct water from the roots to the leaves and to store up and give back according to the season the reserves prepared in the leaves. By the time they become competent to conduct water, all xylem tracheids and vessels have lost their cytoplasm and the cells are therefore functionally dead. All wood in a tree is first formed as sapwood. The more leaves a tree bears and the more vigorous its growth, the larger the volume of sapwood required. Hence trees making rapid growth in the open have thicker sapwood for their size than trees of the same species growing in dense forests. Sometimes trees (of species that do form heartwood) grown in the open may become of considerable size, 30 cm (12 in) or more in diameter, before any heartwood begins to form, for example, in second growth hickory, or open-grown pines.
No definite relation exists between the annual rings of growth and the amount of sapwood. Within the same species the cross-sectional area of the sapwood is very roughly proportional to the size of the crown of the tree. If the rings are narrow, more of them are required than where they are wide. As the tree gets larger, the sapwood must necessarily become thinner or increase materially in volume. Sapwood is relatively thicker in the upper portion of the trunk of a tree than near the base, because the age and the diameter of the upper sections are less.
When a tree is very young it is covered with limbs almost, if not entirely, to the ground, but as it grows older some or all of them will eventually die and are either broken off or fall off. Subsequent growth of wood may completely conceal the stubs which will remain as knots. No matter how smooth and clear a log is on the outside, it is more or less knotty near the middle. Consequently, the sapwood of an old tree, and particularly of a forest-grown tree, will be freer from knots than the inner heartwood. Since in most uses of wood, knots are defects that weaken the timber and interfere with its ease of working and other properties, it follows that a given piece of sapwood, because of its position in the tree, may well be stronger than a piece of heartwood from the same tree.
Different pieces of wood cut from a large tree may differ decidedly, particularly if the tree is big and mature. In some trees, the wood laid on late in the life of a tree is softer, lighter, weaker, and more even textured than that produced earlier, but in other trees, the reverse applies. This may or may not correspond to heartwood and sapwood. In a large log the sapwood, because of the time in the life of the tree when it was grown, may be inferior in hardness, strength, and toughness to equally sound heartwood from the same log. In a smaller tree, the reverse may be true.
Color
In species which show a distinct difference between heartwood and sapwood the natural color of heartwood is usually darker than that of the sapwood, and very frequently the contrast is conspicuous (see section of yew log above). This is produced by deposits in the heartwood of chemical substances, so that a dramatic color variation does not imply a significant difference in the mechanical properties of heartwood and sapwood, although there may be a marked biochemical difference between the two.
Some experiments on very resinous longleaf pine specimens indicate an increase in strength, due to the resin which increases the strength when dry. Such resin-saturated heartwood is called "fat lighter". Structures built of fat lighter are almost impervious to rot and termites, and very flammable. Tree stumps of old longleaf pines are often dug, split into small pieces and sold as kindling for fires. Stumps thus dug may actually remain a century or more since being cut. Spruce impregnated with crude resin and dried is also greatly increased in strength thereby.
Since the latewood of a growth ring is usually darker in color than the earlywood, this fact may be used in visually judging the density, and therefore the hardness and strength of the material. This is particularly the case with coniferous woods. In ring-porous woods the vessels of the early wood often appear on a finished surface as darker than the denser latewood, though on cross sections of heartwood the reverse is commonly true. Otherwise the color of wood is no indication of strength.
Abnormal discoloration of wood often denotes a diseased condition, indicating unsoundness. The black check in western hemlock is the result of insect attacks. The reddish-brown streaks so common in hickory and certain other woods are mostly the result of injury by birds. The discoloration is merely an indication of an injury, and in all probability does not of itself affect the properties of the wood. Certain rot-producing fungi impart to wood characteristic colors which thus become symptomatic of weakness. Ordinary sap-staining is due to fungal growth, but does not necessarily produce a weakening effect.
Water content
Water occurs in living wood in three locations, namely:
- in the cell walls
- in the protoplasmic contents of the cells
- as free water in the cell cavities and spaces, especially of the xylem
In heartwood it occurs only in the first and last forms. Wood that is thoroughly air-dried (in equilibrium with the moisture content of the air) retains 8–16% of the water in the cell walls, and none, or practically none, in the other forms. Even oven-dried wood retains a small percentage of moisture, but for all except chemical purposes, may be considered absolutely dry.
The general effect of the water content upon the wood substance is to render it softer and more pliable. A similar effect occurs in the softening action of water on rawhide, paper, or cloth. Within certain limits, the greater the water content, the greater its softening effect. The moisture in wood can be measured by several different moisture meters.
Drying produces a decided increase in the strength of wood, particularly in small specimens. An extreme example is the case of a completely dry spruce block 5 cm in section, which will sustain a permanent load four times as great as a green (undried) block of the same size will.
The greatest strength increase due to drying is in the ultimate crushing strength, and strength at elastic limit in endwise compression; these are followed by the modulus of rupture, and stress at elastic limit in cross-bending, while the modulus of elasticity is least affected.
Structure
Wood is a heterogeneous, hygroscopic, cellular and anisotropic (or more specifically, orthotropic) material. It consists of cells, and the cell walls are composed of micro-fibrils of cellulose (40–50%) and hemicellulose (15–25%) impregnated with lignin (15–30%).
In coniferous or softwood species the wood cells are mostly of one kind, tracheids, and as a result the material is much more uniform in structure than that of most hardwoods. There are no vessels ("pores") in coniferous wood such as one sees so prominently in oak and ash, for example.
The structure of hardwoods is more complex. The water conducting capability is mostly taken care of by vessels: in some cases (oak, chestnut, ash) these are quite large and distinct, in others (buckeye, poplar, willow) too small to be seen without a hand lens. In discussing such woods it is customary to divide them into two large classes, ring-porous and diffuse-porous.
In ring-porous species, such as ash, black locust, catalpa, chestnut, elm, hickory, mulberry, and oak, the larger vessels or pores (as cross sections of vessels are called) are localized in the part of the growth ring formed in spring, thus forming a region of more or less open and porous tissue. The rest of the ring, produced in summer, is made up of smaller vessels and a much greater proportion of wood fibers. These fibers are the elements which give strength and toughness to wood, while the vessels are a source of weakness.
In diffuse-porous woods the pores are evenly sized so that the water conducting capability is scattered throughout the growth ring instead of being collected in a band or row. Examples of this kind of wood are alder, basswood, birch, buckeye, maple, willow, and the Populus species such as aspen, cottonwood and poplar. Some species, such as walnut and cherry, are on the border between the two classes, forming an intermediate group.
Earlywood and latewood
In softwood
In temperate softwoods, there often is a marked difference between latewood and earlywood. The latewood will be denser than that formed early in the season. When examined under a microscope, the cells of dense latewood are seen to be very thick-walled and with very small cell cavities, while those formed first in the season have thin walls and large cell cavities. The strength is in the walls, not the cavities. Hence the greater the proportion of latewood, the greater the density and strength. In choosing a piece of pine where strength or stiffness is the important consideration, the principal thing to observe is the comparative amounts of earlywood and latewood. The width of ring is not nearly so important as the proportion and nature of the latewood in the ring.
If a heavy piece of pine is compared with a lightweight piece it will be seen at once that the heavier one contains a larger proportion of latewood than the other, and is therefore showing more clearly demarcated growth rings. In white pines there is not much contrast between the different parts of the ring, and as a result the wood is very uniform in texture and is easy to work. In hard pines, on the other hand, the latewood is very dense and is deep-colored, presenting a very decided contrast to the soft, straw-colored earlywood.
It is not only the proportion of latewood, but also its quality, that counts. In specimens that show a very large proportion of latewood it may be noticeably more porous and weigh considerably less than the latewood in pieces that contain less latewood. One can judge comparative density, and therefore to some extent strength, by visual inspection.
No satisfactory explanation can as yet be given for the exact mechanisms determining the formation of earlywood and latewood. Several factors may be involved. In conifers, at least, rate of growth alone does not determine the proportion of the two portions of the ring, for in some cases the wood of slow growth is very hard and heavy, while in others the opposite is true. The quality of the site where the tree grows undoubtedly affects the character of the wood formed, though it is not possible to formulate a rule governing it. In general, where strength or ease of working is essential, woods of moderate to slow growth should be chosen.
In ring-porous woods
In ring-porous woods, each season's growth is always well defined, because the large pores formed early in the season abut on the denser tissue of the year before.
In the case of the ring-porous hardwoods, there seems to exist a pretty definite relation between the rate of growth of timber and its properties. This may be briefly summed up in the general statement that the more rapid the growth or the wider the rings of growth, the heavier, harder, stronger, and stiffer the wood. This, it must be remembered, applies only to ring-porous woods such as oak, ash, hickory, and others of the same group, and is, of course, subject to some exceptions and limitations.
In ring-porous woods of good growth, it is usually the latewood in which the thick-walled, strength-giving fibers are most abundant. As the breadth of ring diminishes, this latewood is reduced so that very slow growth produces comparatively light, porous wood composed of thin-walled vessels and wood parenchyma. In good oak, these large vessels of the earlywood occupy from six to ten percent of the volume of the log, while in inferior material they may make up 25% or more. The latewood of good oak is dark colored and firm, and consists mostly of thick-walled fibers which form one-half or more of the wood. In inferior oak, this latewood is much reduced both in quantity and quality. Such variation is very largely the result of rate of growth.
Wide-ringed wood is often called "second-growth", because the growth of the young timber in open stands after the old trees have been removed is more rapid than in trees in a closed forest, and in the manufacture of articles where strength is an important consideration such "second-growth" hardwood material is preferred. This is particularly the case in the choice of hickory for handles and spokes. Here not only strength, but toughness and resilience are important.
The results of a series of tests on hickory by the U.S. Forest Service show that:
- "The work or shock-resisting ability is greatest in wide-ringed wood that has from 5 to 14 rings per inch (rings 1.8-5 mm thick), is fairly constant from 14 to 38 rings per inch (rings 0.7–1.8 mm thick), and decreases rapidly from 38 to 47 rings per inch (rings 0.5–0.7 mm thick). The strength at maximum load is not so great with the most rapid-growing wood; it is maximum with from 14 to 20 rings per inch (rings 1.3–1.8 mm thick), and again becomes less as the wood becomes more closely ringed. The natural deduction is that wood of first-class mechanical value shows from 5 to 20 rings per inch (rings 1.3–5 mm thick) and that slower growth yields poorer stock. Thus the inspector or buyer of hickory should discriminate against timber that has more than 20 rings per inch (rings less than 1.3 mm thick). Exceptions exist, however, in the case of normal growth upon dry situations, in which the slow-growing material may be strong and tough."
The effect of rate of growth on the qualities of chestnut wood is summarized by the same authority as follows:
- "When the rings are wide, the transition from spring wood to summer wood is gradual, while in the narrow rings the spring wood passes into summer wood abruptly. The width of the spring wood changes but little with the width of the annual ring, so that the narrowing or broadening of the annual ring is always at the expense of the summer wood. The narrow vessels of the summer wood make it richer in wood substance than the spring wood composed of wide vessels. Therefore, rapid-growing specimens with wide rings have more wood substance than slow-growing trees with narrow rings. Since the more the wood substance the greater the weight, and the greater the weight the stronger the wood, chestnuts with wide rings must have stronger wood than chestnuts with narrow rings. This agrees with the accepted view that sprouts (which always have wide rings) yield better and stronger wood than seedling chestnuts, which grow more slowly in diameter."
In diffuse-porous woods
In the diffuse-porous woods, the demarcation between rings is not always so clear and in some cases is almost (if not entirely) invisible to the unaided eye. Conversely, when there is a clear demarcation there may not be a noticeable difference in structure within the growth ring.
In diffuse-porous woods, as has been stated, the vessels or pores are even-sized, so that the water conducting capability is scattered throughout the ring instead of collected in the earlywood. The effect of rate of growth is, therefore, not the same as in the ring-porous woods, approaching more nearly the conditions in the conifers. In general, it may be stated that such woods of medium growth afford stronger material than when very rapidly or very slowly grown. In many uses of wood, total strength is not the main consideration. If ease of working is prized, wood should be chosen with regard to its uniformity of texture and straightness of grain, which will in most cases occur when there is little contrast between the latewood of one season's growth and the earlywood of the next.
Monocots
Structural material that resembles ordinary, "dicot" or conifer timber in its gross handling characteristics is produced by a number of monocot plants, and these also are colloquially called wood. Of these, bamboo, botanically a member of the grass family, has considerable economic importance, larger culms being widely used as a building and construction material and in the manufacture of engineered flooring, panels and veneer. Another major plant group that produces material that often is called wood are the palms. Of much less importance are plants such as Pandanus, Dracaena and Cordyline. With all this material, the structure and composition of the processed raw material is quite different from ordinary wood.
Specific gravity
The single most revealing property of wood as an indicator of wood quality is specific gravity (Timell 1986), as both pulp yield and lumber strength are determined by it. Specific gravity is the ratio of the mass of a substance to the mass of an equal volume of water; density is the ratio of a mass of a quantity of a substance to the volume of that quantity and is expressed in mass per unit substance, e.g., grams per milliliter (g/cm or g/ml). The terms are essentially equivalent as long as the metric system is used. Upon drying, wood shrinks and its density increases. Minimum values are associated with green (water-saturated) wood and are referred to as basic specific gravity (Timell 1986).
The U.S. Forest Products Laboratory lists a variety of ways to define specific gravity (G) and density (ρ) for wood:
Symbol | Mass basis | Volume basis |
---|---|---|
G0 | Ovendry | Ovendry |
Gb (basic) | Ovendry | Green |
G12 | Ovendry | 12% MC |
Gx | Ovendry | x% MC |
ρ0 | Ovendry | Ovendry |
ρ12 | 12% MC | 12% MC |
ρx | x% MC | x% MC |
The FPL has adopted Gb and G12 for specific gravity, in accordance with the ASTM D2555 standard. These are scientifically useful, but don't represent any condition that could physically occur. The FPL Wood Handbook also provides formulas for approximately converting any of these measurements to any other.
Density
See also: Janka hardness testWood density is determined by multiple growth and physiological factors compounded into "one fairly easily measured wood characteristic" (Elliott 1970).
Age, diameter, height, radial (trunk) growth, geographical location, site and growing conditions, silvicultural treatment, and seed source all to some degree influence wood density. Variation is to be expected. Within an individual tree, the variation in wood density is often as great as or even greater than that between different trees (Timell 1986). Variation of specific gravity within the bole of a tree can occur in either the horizontal or vertical direction.
Because the specific gravity as defined above uses an unrealistic condition, woodworkers tend to use the "average dried weight", which is a density based on mass at 12% moisture content and volume at the same (ρ12). This condition occurs when the wood is at equilibrium moisture content with air at about 65% relative humidity and temperature at 30 °C (86 °F). This density is expressed in units of kg/m or lbs/ft.
Tables
The following tables list the mechanical properties of wood and lumber plant species, including bamboo. See also Mechanical properties of tonewoods for additional properties.
Wood properties:
Common name | Scientific name | Moisture content | Density (kg/m) | Compressive strength (megapascals) | Flexural strength (megapascals) |
---|---|---|---|---|---|
Red Alder | Alnus rubra | Green | 370 | 20.4 | 45 |
Red Alder | Alnus rubra | 12.00% | 410 | 40.1 | 68 |
Black Ash | Fraxinus nigra | Green | 450 | 15.9 | 41 |
Black Ash | Fraxinus nigra | 12.00% | 490 | 41.2 | 87 |
Blue Ash | Fraxinus quadrangulata | Green | 530 | 24.8 | 66 |
Blue Ash | Fraxinus quadrangulata | 12.00% | 580 | 48.1 | 95 |
Green Ash | Fraxinus pennsylvanica | Green | 530 | 29 | 66 |
Green Ash | Fraxinus pennsylvanica | 12.00% | 560 | 48.8 | 97 |
Oregon Ash | Fraxinus latifolia | Green | 500 | 24.2 | 52 |
Oregon Ash | Fraxinus latifolia | 12.00% | 550 | 41.6 | 88 |
White Ash | Fraxinus americana | Green | 550 | 27.5 | 66 |
White Ash | Fraxinus americana | 12.00% | 600 | 51.1 | 103 |
Bigtooth Aspen | Populus grandidentata | Green | 360 | 17.2 | 37 |
Bigtooth Aspen | Populus grandidentata | 12.00% | 390 | 36.5 | 63 |
Quaking Aspen | Populus tremuloides | Green | 350 | 14.8 | 35 |
Quaking Aspen | Populus tremuloides | 12.00% | 380 | 29.3 | 58 |
American Basswood | Tilia americana | Green | 320 | 15.3 | 34 |
American Basswood | Tilia americana | 12.00% | 370 | 32.6 | 60 |
American Beech | Fagus grandifolia | Green | 560 | 24.5 | 59 |
American Beech | Fagus grandifolia | 12.00% | 640 | 50.3 | 103 |
Paper Birch | Betula papyrifera | Green | 480 | 16.3 | 44 |
Paper Birch | Betula papyrifera | 12.00% | 550 | 39.2 | 85 |
Sweet Birch | Betula lenta | Green | 600 | 25.8 | 65 |
Sweet Birch | Betula lenta | 12.00% | 650 | 58.9 | 117 |
Yellow Birch | Betula alleghaniensis | Green | 550 | 23.3 | 57 |
Yellow Birch | Betula alleghaniensis | 12.00% | 620 | 56.3 | 114 |
Butternut | Juglans cinerea | Green | 360 | 16.7 | 37 |
Butternut | Juglans cinerea | 12.00% | 380 | 36.2 | 56 |
Black Cherry | Prunus serotina | Green | 470 | 24.4 | 55 |
Blach Cherry | Prunus serotina | 12.00% | 500 | 49 | 85 |
American Chestnut | Castanea dentata | Green | 400 | 17 | 39 |
American Chestnut | Castanea dentata | 12.00% | 430 | 36.7 | 59 |
Balsam Poplar Cottonwood | Populus balsamifera | Green | 310 | 11.7 | 27 |
Balsam Poplar Cottonwood | Populus balsamifera | 12.00% | 340 | 27.7 | 47 |
Black Cottonwood | Populus trichocarpa | Green | 310 | 15.2 | 34 |
Black Cottonwood | Populus trichocarpa | 12.00% | 350 | 31 | 59 |
Eastern Cottonwood | Populus deltoides | Green | 370 | 15.7 | 37 |
Eastern Cottonwood | Populus deltoides | 12.00% | 400 | 33.9 | 59 |
American Elm | Ulmus americana | Green | 460 | 20.1 | 50 |
American Elm | Ulmus americana | 12.00% | 500 | 38.1 | 81 |
Rock Elm | Ulmus thomasii | Green | 570 | 26.1 | 66 |
Rock Elm | Ulmus thomasii | 12.00% | 630 | 48.6 | 102 |
Slippery Elm | Ulmus rubra | Green | 480 | 22.9 | 55 |
Slippery Elm | Ulmus rubra | 12.00% | 530 | 43.9 | 90 |
Hackberry | Celtis occidentalis | Green | 490 | 18.3 | 45 |
Hackberry | Celtis occidentalis | 12.00% | 530 | 37.5 | 76 |
Bitternut Hickory | Carya cordiformis | Green | 600 | 31.5 | 71 |
Bitternut Hickory | Carya cordiformis | 12.00% | 660 | 62.3 | 118 |
Nutmeg Hickory | Carya myristiciformis | Green | 560 | 27.4 | 63 |
Nutmeg Hickory | Carya myristiciformis | 12.00% | 600 | 47.6 | 114 |
Pecan Hickory | Carya illinoinensis | Green | 600 | 27.5 | 68 |
Pecan Hickory | Carya illinoinensis | 12.00% | 660 | 54.1 | 94 |
Water Hickory | Carya aquatica | Green | 610 | 32.1 | 74 |
Water Hickory | Carya aquatica | 12.00% | 620 | 59.3 | 123 |
Mockernut Hickory | Carya tomentosa | Green | 640 | 30.9 | 77 |
Mockernut Hickory | Carya tomentosa | 12.00% | 720 | 61.6 | 132 |
Pignut Hickory | Carya glabra | Green | 660 | 33.2 | 81 |
Pignut Hickory | Carya glabra | 12.00% | 750 | 63.4 | 139 |
Shagbark Hickory | Carya ovata | Green | 640 | 31.6 | 76 |
Shagbark Hickory | Carya ovata | 12.00% | 720 | 63.5 | 139 |
Shellbark Hickory | Carya laciniosa | Green | 620 | 27 | 72 |
Shellbark Hickory | Carya laciniosa | 12.00% | 690 | 55.2 | 125 |
Honeylocust | Gleditsia triacanthos | Green | 600 | 30.5 | 70 |
Honeylocust | Gleditsia triacanthos | 12.00% | 600 | 51.7 | 101 |
Black Locust | Robinia pseudoacacia | Green | 660 | 46.9 | 95 |
Black Locust | Robinia pseudoacacia | 12.00% | 690 | 70.2 | 134 |
Cucumber Tree Magnolia | Magnolia acuminata | Green | 440 | 21.6 | 51 |
Cucumber Tree Magnolia | Magnolia acuminata | 12.00% | 480 | 43.5 | 85 |
Southern Magnolia | Magnolia grandiflora | Green | 460 | 18.6 | 47 |
Southern Magnolia | Magnolia grandiflora | 12.00% | 500 | 37.6 | 77 |
Bigleaf Maple | Acer macrophyllum | Green | 440 | 22.3 | 51 |
Bigleaf Maple | Acer macrophyllum | 12.00% | 480 | 41 | 74 |
Black Maple | Acer nigrum | Green | 520 | 22.5 | 54 |
Black Maple | Acer nigrum | 12.00% | 570 | 46.1 | 92 |
Red Maple | Acer rubrum | Green | 490 | 22.6 | 53 |
Red Maple | Acer rubrum | 12.00% | 540 | 45.1 | 92 |
Silver Maple | Acer saccharinum | Green | 440 | 17.2 | 40 |
Silver Maple | Acer saccharinum | 12.00% | 470 | 36 | 61 |
Sugar Maple | Acer saccharum | Green | 560 | 27.7 | 65 |
Sugar Maple | Acer saccharum | 12.00% | 630 | 54 | 109 |
Black Red Oak | Quercus velutina | Green | 560 | 23.9 | 57 |
Black Red Oak | Quercus velutina | 12.00% | 610 | 45 | 96 |
Cherrybark Red Oak | Quercus pagoda | Green | 610 | 31.9 | 74 |
Cherrybark Red Oak | Quercus pagoda | 12.00% | 680 | 60.3 | 125 |
Laurel Red Oak | Quercus hemisphaerica | Green | 560 | 21.9 | 54 |
Laurel Red Oak | Quercus hemisphaerica | 12.00% | 630 | 48.1 | 87 |
Northern Red Oak | Quercus rubra | Green | 560 | 23.7 | 57 |
Northern Red Oak | Quercus rubra | 12.00% | 630 | 46.6 | 99 |
Pin Red Oak | Quercus palustris | Green | 580 | 25.4 | 57 |
Pin Red Oak | Quercus palustris | 12.00% | 630 | 47 | 97 |
Scarlet Red Oak | Quercus coccinea | Green | 600 | 28.2 | 72 |
Scarlet Red Oak | Quercus coccinea | 12.00% | 670 | 57.4 | 120 |
Southern Red Oak | Quercus falcata | Green | 520 | 20.9 | 48 |
Southern Red Oak | Quercus falcata | 12.00% | 590 | 42 | 75 |
Water Red Oak | Quercus nigra | Green | 560 | 25.8 | 61 |
Water Red Oak | Quercus nigra | 12.00% | 630 | 46.7 | 106 |
Willow Red Oak | Quercus phellos | Green | 560 | 20.7 | 51 |
Willow Red Oak | Quercus phellos | 12.00% | 690 | 48.5 | 100 |
Bur White Oak | Quercus macrocarpa | Green | 580 | 22.7 | 50 |
Bur White Oak | Quercus macrocarpa | 12.00% | 640 | 41.8 | 71 |
Chestnut White Oak | Quercus montana | Green | 570 | 24.3 | 55 |
Chestnut White Oak | Quercus montana | 12.00% | 660 | 47.1 | 92 |
Live White Oak | Quercus virginiana | Green | 800 | 37.4 | 82 |
Live White Oak | Quercus virginiana | 12.00% | 880 | 61.4 | 127 |
Overcup White Oak | Quercus lyrata | Green | 570 | 23.2 | 55 |
Overcup White Oak | Quercus lyrata | 12.00% | 630 | 42.7 | 87 |
Post White Oak | Quercus stellata | Green | 600 | 24 | 56 |
Post White Oak | Quercus stellata | 12.00% | 670 | 45.3 | 91 |
Swamp Chestnut White Oak | Quercus michauxii | Green | 600 | 24.4 | 59 |
Swamp Chestnut White Oak | Quercus michauxii | 12.00% | 670 | 50.1 | 96 |
Swamp White Oak | Quercus bicolor | Green | 640 | 30.1 | 68 |
Swamp White Oak | Quercus bicolor | 12.00% | 720 | 59.3 | 122 |
White Oak | Quercus alba | Green | 600 | 24.5 | 57 |
White Oak | Quercus alba | 12.00% | 680 | 51.3 | 105 |
Sassafras | Sassafras albidum | Green | 420 | 18.8 | 41 |
Sassafras | Sassafras albidum | 12.00% | 460 | 32.8 | 62 |
Sweetgum | Liquidambar styraciflua | Green | 460 | 21 | 49 |
Sweetgum | Liquidambar styraciflua | 12.00% | 520 | 43.6 | 86 |
American Sycamore | Platanus occidentalis | Green | 460 | 20.1 | 45 |
American Sycamore | Platanus occidentalis | 12.00% | 490 | 37.1 | 69 |
Tanoak | Notholithocarpus densiflorus | Green | 580 | 32.1 | 72 |
Tanoak | Notholithocarpus densiflorus | 12.00% | 580 | 32.1 | 72 |
Black Tupelo | Nyssa sylvatica | Green | 460 | 21 | 48 |
Black Tupelo | Nyssa sylvatica | 12.00% | 500 | 38.1 | 66 |
Water Tupelo | Nyssa aquatica | Green | 460 | 23.2 | 50 |
Water Tupelo | Nyssa aquatica | 12.00% | 500 | 40.8 | 66 |
Black Walnut | Juglans nigra | Green | 510 | 29.6 | 66 |
Black Walnut | Juglans nigra | 12.00% | 550 | 52.3 | 101 |
Black Willow | Salix nigra | Green | 360 | 14.1 | 33 |
Black Willow | Salix nigra | 12.00% | 390 | 28.3 | 54 |
Yellow Poplar | Liriodendron tulipifera | Green | 400 | 18.3 | 41 |
Yellow Poplar | Liriodendron tulipifera | 12.00% | 420 | 38.2 | 70 |
Baldcypress | Taxodium distichum | Green | 420 | 24.7 | 46 |
Baldcypress | Taxodium distichum | 12.00% | 460 | 43.9 | 73 |
Atlantic White Cedar | Chamaecyparis thyoides | Green | 310 | 16.5 | 32 |
Atlantic White Cedar | Chamaecyparis thyoides | 12.00% | 320 | 32.4 | 47 |
Eastern Redcedar | Juniperus virginiana | Green | 440 | 24.6 | 48 |
Eastern Redcedar | Juniperus virginiana | 12.00% | 470 | 41.5 | 61 |
Incense Cedar | Calocedrus decurrens | Green | 350 | 21.7 | 43 |
Incense Cedar | Calocedrus decurrens | 12.00% | 370 | 35.9 | 55 |
Northern White Cedar | Thuja occidentalis | Green | 290 | 13.7 | 29 |
Northern White Cedar | Thuja occidentalis | 12.00% | 310 | 27.3 | 45 |
Port Orford Cedar | Chamaecyparis lawsoniana | Green | 390 | 21.6 | 45 |
Port Orford Cedar | Chamaecyparis lawsoniana | 12.00% | 430 | 43.1 | 88 |
Western Redcedar | Thuja plicata | Green | 310 | 19.1 | 35.9 |
Western Redcedar | Thuja plicata | 12.00% | 320 | 31.4 | 51.7 |
Yellow Cedar | Cupressus nootkatensis | Green | 420 | 21 | 44 |
Yellow Cedar | Cupressus nootkatensis | 12.00% | 440 | 43.5 | 77 |
Coast Douglas Fir | Pseudotsuga menziesii var. menziesii | Green | 450 | 26.1 | 53 |
Coast Douglas Fir | Pseudotsuga menziesii var. menziesii | 12.00% | 480 | 49.9 | 85 |
Interior West Douglas Fir | Pseudotsuga Menziesii | Green | 460 | 26.7 | 53 |
Interior West Douglas Fir | Pseudotsuga Menziesii | 12.00% | 500 | 51.2 | 87 |
Interior North Douglas Fir | Pseudotsuga menziesii var. glauca | Green | 450 | 23.9 | 51 |
Interior North Douglas Fir | Pseudotsuga menziesii var. glauca | 12.00% | 480 | 47.6 | 90 |
Interior South Douglas Fir | Pseudotsuga lindleyana | Green | 430 | 21.4 | 47 |
Interior South Douglas Fir | Pseudotsuga lindleyana | 12.00% | 460 | 43 | 82 |
Balsam Fir | Abies balsamea | Green | 330 | 18.1 | 38 |
Balsam Fir | Abies balsamea | 12.00% | 350 | 36.4 | 63 |
California Red Fir | Abies magnifica | Green | 360 | 19 | 40 |
California Red Fir | Abies magnifica | 12.00% | 380 | 37.6 | 72.4 |
Grand Fir | Abies grandis | Green | 350 | 20.3 | 40 |
Grand Fir | Abies grandis | 12.00% | 370 | 36.5 | 61.4 |
Noble Fir | Abies procera | Green | 370 | 20.8 | 43 |
Noble Fir | Abies procera | 12.00% | 390 | 42.1 | 74 |
Pacific Silver Fir | Abies amabilis | Green | 400 | 21.6 | 44 |
Pacific Silver Fir | Abies amabilis | 12.00% | 430 | 44.2 | 75 |
Subalpine Fir | Abies lasiocarpa | Green | 310 | 15.9 | 34 |
Subalpine Fir | Abies lasiocarpa | 12.00% | 320 | 33.5 | 59 |
White Fir | Abies concolor | Green | 370 | 20 | 41 |
White Fir | Abies concolor | 12.00% | 390 | 40 | 68 |
Eastern Hemlock | Tsuga canadensis | Green | 380 | 21.2 | 44 |
Eastern Hemlock | Tsuga canadensis | 12.00% | 400 | 37.3 | 61 |
Mountain Hemlock | Tsuga mertensiana | Green | 420 | 19.9 | 43 |
Mountain Hemlock | Tsuga mertensiana | 12.00% | 450 | 44.4 | 79 |
Western Hemlock | Tsuga heterophylla | Green | 420 | 23.2 | 46 |
Western Hemlock | Tsuga heterophylla | 12.00% | 450 | 49 | 78 |
Western Larch | Larix occidentalis | Green | 480 | 25.9 | 53 |
Western Larch | Larix occidentalis | 12.00% | 520 | 52.5 | 90 |
Eastern White Pine | Pinus strobus | Green | 340 | 16.8 | 34 |
Eastern White Pine | Pinus strobus | 12.00% | 350 | 33.1 | 59 |
Jack Pine | Pinus banksiana | Green | 400 | 20.3 | 41 |
Jack Pine | Pinus banksiana | 12.00% | 430 | 39 | 68 |
Loblolly Pine | Pinus taeda | Green | 470 | 24.2 | 50 |
Loblolly Pine | Pinus taeda | 12.00% | 510 | 49.2 | 88 |
Lodgepole Pine | Pinus contorta | Green | 380 | 18 | 38 |
Lodgepole Pine | Pinus contorta | 12.00% | 410 | 37 | 65 |
Longleaf Pine | Pinus palustris | Green | 540 | 29.8 | 59 |
Longleaf Pine | Pinus palustris | 12.00% | 590 | 58.4 | 100 |
Pitch Pine | Pinus rigida | Green | 470 | 20.3 | 47 |
Pitch Pine | Pinus rigida | 12.00% | 520 | 41 | 74 |
Pond Pine | Pinus serotina | Green | 510 | 25.2 | 51 |
Pond Pine | Pinus serotina | 12.00% | 560 | 52 | 80 |
Ponderosa Pine | Pinus ponderosa | Green | 380 | 16.9 | 35 |
Ponderosa Pine | Pinus ponderosa | 12.00% | 400 | 36.7 | 65 |
Red Pine | Pinus resinosa | Green | 410 | 18.8 | 40 |
Red Pine | Pinus resinosa | 12.00% | 460 | 41.9 | 76 |
Sand Pine | Pinus clausa | Green | 460 | 23.7 | 52 |
Sand Pine | Pinus clausa | 12.00% | 480 | 47.7 | 80 |
Shortleaf Pine | Pinus echinata | Green | 470 | 24.3 | 51 |
Shortleaf Pine | Pinus echinata | 12.00% | 510 | 50.1 | 90 |
Slash Pine | Pinus elliottii | Green | 540 | 26.3 | 60 |
Slash Pine | Pinus elliottii | 12.00% | 590 | 56.1 | 112 |
Spruce Pine | Pinus glabra | Green | 410 | 19.6 | 41 |
Spruce Pine | Pinus glabra | 12.00% | 440 | 39 | 72 |
Sugar Pine | Pinus lambertiana | Green | 340 | 17 | 34 |
Sugar Pine | Pinus lambertiana | 12.00% | 360 | 30.8 | 57 |
Virginia Pine | Pinus virginiana | Green | 450 | 23.6 | 50 |
Virginia Pine | Pinus virginiana | 12.00% | 480 | 46.3 | 90 |
Western White Pine | Pinus monticola | Green | 360 | 16.8 | 32 |
Western White Pine | Pinus monticola | 12.00% | 380 | 34.7 | 67 |
Redwood Old Growth | Sequoia sempervirens | Green | 380 | 29 | 52 |
Redwood Old Growth | Sequoia sempervirens | 12.00% | 400 | 42.4 | 69 |
Redwood New Growth | Sequoia sempervirens | Green | 340 | 21.4 | 41 |
Redwood New Growth | Sequoia sempervirens | 12.00% | 350 | 36 | 54 |
Black Spruce | Picea mariana | Green | 380 | 19.6 | 42 |
Black Spruce | Picea mariana | 12.00% | 460 | 41.1 | 74 |
Engelmann Spruce | Picea engelmannii | Green | 330 | 15 | 32 |
Engelmann Spruce | Picea engelmannii | 12.00% | 350 | 30.9 | 64 |
Red Spruce | Picea rubens | Green | 370 | 18.8 | 41 |
Red Spruce | Picea rubens | 12.00% | 400 | 38.2 | 74 |
Sitka Spruce | Picea sitchensis | Green | 330 | 16.2 | 34 |
Sitka Spruce | Picea sitchensis | 12.00% | 360 | 35.7 | 65 |
White Spruce | Picea glauca | Green | 370 | 17.7 | 39 |
White Spruce | Picea glauca | 12.00% | 400 | 37.7 | 68 |
Tamarack Spruce | Larix laricina | Green | 490 | 24 | 50 |
Tamarack Spruce | Larix laricina | 12.00% | 530 | 49.4 | 80 |
Bamboo properties:
Common name | Scientific name | Moisture content | Density (kg/m) | Compressive strength (megapascals) | Flexural strength (megapascals) |
---|---|---|---|---|---|
Balku bans | Bambusa balcooa | green | 45 | 73.7 | |
Balku bans | Bambusa balcooa | air dry | 54.15 | 81.1 | |
Balku bans | Bambusa balcooa | 8.5 | 820 | 69 | 151 |
Indian thorny bamboo | Bambusa bambos | 9.5 | 710 | 61 | 143 |
Indian thorny bamboo | Bambusa bambos | 43.05 | 37.15 | ||
Nodding Bamboo | Bambusa nutans | 8 | 890 | 75 | 52.9 |
Nodding Bamboo | Bambusa nutans | 87 | 46 | 52.4 | |
Nodding Bamboo | Bambusa nutans | 12 | 85 | 67.5 | |
Nodding Bamboo | Bambusa nutans | 88.3 | 44.7 | 88 | |
Nodding Bamboo | Bambusa nutans | 14 | 47.9 | 216 | |
Clumping Bamboo | Bambusa pervariabilis | 45.8 | |||
Clumping Bamboo | Bambusa pervariabilis | 5 | 79 | 80 | |
Clumping Bamboo | Bambusa pervariabilis | 20 | 35 | 37 | |
Burmese bamboo | Bambusa polymorpha | 95.1 | 32.1 | 28.3 | |
Bambusa spinosa | air dry | 57 | 51.77 | ||
Indian timber bamboo | Bambusa tulda | 73.6 | 40.7 | 51.1 | |
Indian timber bamboo | Bambusa tulda | 11.9 | 68 | 66.7 | |
Indian timber bamboo | Bambusa tulda | 8.6 | 910 | 79 | 194 |
dragon bamboo | Dendrocalamus giganteus | 8 | 740 | 70 | 193 |
Hamilton's bamboo | Dendrocalamus hamiltonii | 8.5 | 590 | 70 | 89 |
White bamboo | Dendrocalamus membranaceus | 102 | 40.5 | 26.3 | |
String Bamboo | Gigantochloa apus | 54.3 | 24.1 | 102 | |
String Bamboo | Gigantochloa apus | 15.1 | 37.95 | 87.5 | |
Java Black Bamboo | Gigantochloa atroviolacea | 54 | 23.8 | 92.3 | |
Java Black Bamboo | Gigantochloa atroviolacea | 15 | 35.7 | 94.1 | |
Giant Atter | Gigantochloa atter | 72.3 | 26.4 | 98 | |
Giant Atter | Gigantochloa atter | 14.4 | 31.95 | 122.7 | |
Gigantochloa macrostachya | 8 | 960 | 71 | 154 | |
American Narrow-Leaved Bamboo | Guadua angustifolia | 42 | 53.5 | ||
American Narrow-Leaved Bamboo | Guadua angustifolia | 63.6 | 144.8 | ||
American Narrow-Leaved Bamboo | Guadua angustifolia | 86.3 | 46 | ||
American Narrow-Leaved Bamboo | Guadua angustifolia | 77.5 | 82 | ||
American Narrow-Leaved Bamboo | Guadua angustifolia | 15 | 56 | 87 | |
American Narrow-Leaved Bamboo | Guadua angustifolia | 63.3 | |||
American Narrow-Leaved Bamboo | Guadua angustifolia | 28 | |||
American Narrow-Leaved Bamboo | Guadua angustifolia | 56.2 | |||
American Narrow-Leaved Bamboo | Guadua angustifolia | 38 | |||
Berry Bamboo | Melocanna baccifera | 12.8 | 69.9 | 57.6 | |
Japanese timber bamboo | Phyllostachys bambusoides | 51 | |||
Japanese timber bamboo | Phyllostachys bambusoides | 8 | 730 | 63 | |
Japanese timber bamboo | Phyllostachys bambusoides | 64 | 44 | ||
Japanese timber bamboo | Phyllostachys bambusoides | 61 | 40 | ||
Japanese timber bamboo | Phyllostachys bambusoides | 9 | 71 | ||
Japanese timber bamboo | Phyllostachys bambusoides | 9 | 74 | ||
Japanese timber bamboo | Phyllostachys bambusoides | 12 | 54 | ||
Tortoise shell bamboo | Phyllostachys edulis | 44.6 | |||
Tortoise shell bamboo | Phyllostachys edulis | 75 | 67 | ||
Tortoise shell bamboo | Phyllostachys edulis | 15 | 71 | ||
Tortoise shell bamboo | Phyllostachys edulis | 6 | 108 | ||
Tortoise shell bamboo | Phyllostachys edulis | 0.2 | 147 | ||
Tortoise shell bamboo | Phyllostachys edulis | 5 | 117 | 51 | |
Tortoise shell bamboo | Phyllostachys edulis | 30 | 44 | 55 | |
Tortoise shell bamboo | Phyllostachys edulis | 12.5 | 603 | 60.3 | |
Tortoise shell bamboo | Phyllostachys edulis | 10.3 | 530 | 83 | |
Early Bamboo | Phyllostachys praecox | 28.5 | 827 | 79.3 | |
Oliveri | Thyrsostachys oliveri | 53 | 46.9 | 61.9 | |
Oliveri | Thyrsostachys oliveri | 7.8 | 58 | 90 |
Hard versus soft
It is common to classify wood as either softwood or hardwood. The wood from conifers (e.g. pine) is called softwood, and the wood from dicotyledons (usually broad-leaved trees, e.g. oak) is called hardwood. These names are a bit misleading, as hardwoods are not necessarily hard, and softwoods are not necessarily soft. The well-known balsa (a hardwood) is actually softer than any commercial softwood. Conversely, some softwoods (e.g. yew) are harder than many hardwoods.
There is a strong relationship between the properties of wood and the properties of the particular tree that yielded it, at least for certain species. For example, in loblolly pine, wind exposure and stem position greatly affect the hardness of wood, as well as compression wood content. The density of wood varies with species. The density of a wood correlates with its strength (mechanical properties). For example, mahogany is a medium-dense hardwood that is excellent for fine furniture crafting, whereas balsa is light, making it useful for model building. One of the densest woods is black ironwood.
Chemistry
The chemical composition of wood varies from species to species, but is approximately 50% carbon, 42% oxygen, 6% hydrogen, 1% nitrogen, and 1% other elements (mainly calcium, potassium, sodium, magnesium, iron, and manganese) by weight. Wood also contains sulfur, chlorine, silicon, phosphorus, and other elements in small quantity.
Aside from water, wood has three main components. Cellulose, a crystalline polymer derived from glucose, constitutes about 41–43%. Next in abundance is hemicellulose, which is around 20% in deciduous trees but near 30% in conifers. It is mainly five-carbon sugars that are linked in an irregular manner, in contrast to the cellulose. Lignin is the third component at around 27% in coniferous wood vs. 23% in deciduous trees. Lignin confers the hydrophobic properties reflecting the fact that it is based on aromatic rings. These three components are interwoven, and direct covalent linkages exist between the lignin and the hemicellulose. A major focus of the paper industry is the separation of the lignin from the cellulose, from which paper is made.
In chemical terms, the difference between hardwood and softwood is reflected in the composition of the constituent lignin. Hardwood lignin is primarily derived from sinapyl alcohol and coniferyl alcohol. Softwood lignin is mainly derived from coniferyl alcohol.
Extractives
Aside from the structural polymers, i.e. cellulose, hemicellulose and lignin (lignocellulose), wood contains a large variety of non-structural constituents, composed of low molecular weight organic compounds, called extractives. These compounds are present in the extracellular space and can be extracted from the wood using different neutral solvents, such as acetone. Analogous content is present in the so-called exudate produced by trees in response to mechanical damage or after being attacked by insects or fungi. Unlike the structural constituents, the composition of extractives varies over wide ranges and depends on many factors. The amount and composition of extractives differs between tree species, various parts of the same tree, and depends on genetic factors and growth conditions, such as climate and geography. For example, slower growing trees and higher parts of trees have higher content of extractives. Generally, the softwood is richer in extractives than the hardwood. Their concentration increases from the cambium to the pith. Barks and branches also contain extractives. Although extractives represent a small fraction of the wood content, usually less than 10%, they are extraordinarily diverse and thus characterize the chemistry of the wood species. Most extractives are secondary metabolites and some of them serve as precursors to other chemicals. Wood extractives display different activities, some of them are produced in response to wounds, and some of them participate in natural defense against insects and fungi.
These compounds contribute to various physical and chemical properties of the wood, such as wood color, fragnance, durability, acoustic properties, hygroscopicity, adhesion, and drying. Considering these impacts, wood extractives also affect the properties of pulp and paper, and importantly cause many problems in paper industry. Some extractives are surface-active substances and unavoidably affect the surface properties of paper, such as water adsorption, friction and strength. Lipophilic extractives often give rise to sticky deposits during kraft pulping and may leave spots on paper. Extractives also account for paper smell, which is important when making food contact materials.
Most wood extractives are lipophilic and only a little part is water-soluble. The lipophilic portion of extractives, which is collectively referred as wood resin, contains fats and fatty acids, sterols and steryl esters, terpenes, terpenoids, resin acids, and waxes. The heating of resin, i.e. distillation, vaporizes the volatile terpenes and leaves the solid component – rosin. The concentrated liquid of volatile compounds extracted during steam distillation is called essential oil. Distillation of oleoresin obtained from many pines provides rosin and turpentine.
Most extractives can be categorized into three groups: aliphatic compounds, terpenes and phenolic compounds. The latter are more water-soluble and usually are absent in the resin.
- Aliphatic compounds include fatty acids, fatty alcohols and their esters with glycerol, fatty alcohols (waxes) and sterols (steryl esters). Hydrocarbons, such as alkanes, are also present in the wood. Suberin is a polyester, made of suberin acids and glycerol, mainly found in barks. Fats serve as a source of energy for the wood cells. The most common wood sterol is sitosterol, and less commonly sitostanol, citrostadienol, campesterol or cholesterol.
- The main terpenes occurring in the softwood include mono-, sesqui- and diterpenes. Meanwhile, the terpene composition of the hardwood is considerably different, consisting of triterpenoids, polyprenols and other higher terpenes. Examples of mono-, di- and sesquiterpenes are α- and β-pinenes, 3-carene, β-myrcene, limonene, thujaplicins, α- and β-phellandrenes, α-muurolene, δ-cadinene, α- and δ-cadinols, α- and β-cedrenes, juniperol, longifolene, cis-abienol, borneol, pinifolic acid, nootkatin, chanootin, phytol, geranyl-linalool, β-epimanool, manoyloxide, pimaral and pimarol. Resin acids are usually tricyclic terpenoids, examples of which are pimaric acid, sandaracopimaric acid, isopimaric acid, abietic acid, levopimaric acid, palustric acid, neoabietic acid and dehydroabietic acid. Bicyclic resin acids are also found, such as lambertianic acid, communic acid, mercusic acid and secodehydroabietic acid. Cycloartenol, betulin and squalene are triterpenoids purified from hardwood. Examples of wood polyterpenes are rubber (cis-polypren), gutta percha (trans-polypren), gutta-balatá (trans-polypren) and betulaprenols (acyclic polyterpenoids). The mono- and sesquiterpenes of the softwood are responsible for the typical smell of pine forest. Many monoterpenoids, such as β-myrcene, are used in the preparation of flavors and fragrances. Tropolones, such as hinokitiol and other thujaplicins, are present in decay-resistant trees and display fungicidal and insecticidal properties. Tropolones strongly bind metal ions and can cause digester corrosion in the process kraft pulping. Owing to their metal-binding and ionophoric properties, especially thujaplicins are used in physiology experiments. Different other in-vitro biological activities of thujaplicins have been studied, such as insecticidal, anti-browning, anti-viral, anti-bacterial, anti-fungal, anti-proliferative and anti-oxidant.
- Phenolic compounds are especially found in the hardwood and the bark. The most well-known wood phenolic constituents are stilbenes (e.g. pinosylvin), lignans (e.g. pinoresinol, conidendrin, plicatic acid, hydroxymatairesinol), norlignans (e.g. nyasol, puerosides A and B, hydroxysugiresinol, sequirin-C), tannins (e.g. gallic acid, ellagic acid), flavonoids (e.g. chrysin, taxifolin, catechin, genistein). Most of the phenolic compounds have fungicidal properties and protect the wood from fungal decay. Together with the neolignans the phenolic compounds influence on the color of the wood. Resin acids and phenolic compounds are the main toxic contaminants present in the untreated effluents from pulping. Polyphenolic compounds are one of the most abundant biomolecules produced by plants, such as flavonoids and tannins. Tannins are used in leather industry and have shown to exhibit different biological activities. Flavonoids are very diverse, widely distributed in the plant kingdom and have numerous biological activities and roles.
Uses
Production
Main article: ForestryGlobal production of roundwood rose from 3.5 billion m³ in 2000 to 4 billion m³ in 2021. In 2021, wood fuel was the main product with a 49 percent share of the total (2 billion m³), followed by coniferous industrial roundwood with 30 percent (1.2 billion m³) and non-coniferous industrial roundwood with 21 percent (0.9 billion m³). Asia and the Americas are the two main producing regions, accounting for 29 and 28 percent of the total roundwood production, respectively; Africa and Europe have similar shares of 20–21 percent, while Oceania produces the remaining 2 percent.
Fuel
Main article: Wood fuelWood has a long history of being used as fuel, which continues to this day, mostly in rural areas of the world. Hardwood is preferred over softwood because it creates less smoke and burns longer. Adding a woodstove or fireplace to a home is often felt to add ambiance and warmth.
Pulpwood
Pulpwood is wood that is raised specifically for use in making paper.
Construction
Wood has been an important construction material since humans began building shelters, houses and boats. Nearly all boats were made out of wood until the late 19th century, and wood remains in common use today in boat construction. Elm in particular was used for this purpose as it resisted decay as long as it was kept wet (it also served for water pipe before the advent of more modern plumbing).
Wood to be used for construction work is commonly known as lumber in North America. Elsewhere, lumber usually refers to felled trees, and the word for sawn planks ready for use is timber. In Medieval Europe oak was the wood of choice for all wood construction, including beams, walls, doors, and floors. Today a wider variety of woods is used: solid wood doors are often made from poplar, small-knotted pine, and Douglas fir.
New domestic housing in many parts of the world today is commonly made from timber-framed construction. Engineered wood products are becoming a bigger part of the construction industry. They may be used in both residential and commercial buildings as structural and aesthetic materials.
In buildings made of other materials, wood will still be found as a supporting material, especially in roof construction, in interior doors and their frames, and as exterior cladding.
Wood is also commonly used as shuttering material to form the mold into which concrete is poured during reinforced concrete construction.
Flooring
Main article: Wood flooringA solid wood floor is a floor laid with planks or battens created from a single piece of timber, usually a hardwood. Since wood is hydroscopic (it acquires and loses moisture from the ambient conditions around it) this potential instability effectively limits the length and width of the boards.
Solid hardwood flooring is usually cheaper than engineered timbers and damaged areas can be sanded down and refinished repeatedly, the number of times being limited only by the thickness of wood above the tongue.
Solid hardwood floors were originally used for structural purposes, being installed perpendicular to the wooden support beams of a building (the joists or bearers) and solid construction timber is still often used for sports floors as well as most traditional wood blocks, mosaics and parquetry.
Engineered products
Main article: Engineered woodEngineered wood products, glued building products "engineered" for application-specific performance requirements, are often used in construction and industrial applications. Glued engineered wood products are manufactured by bonding together wood strands, veneers, lumber or other forms of wood fiber with glue to form a larger, more efficient composite structural unit.
These products include glued laminated timber (glulam), wood structural panels (including plywood, oriented strand board and composite panels), laminated veneer lumber (LVL) and other structural composite lumber (SCL) products, parallel strand lumber, and I-joists. Approximately 100 million cubic meters of wood was consumed for this purpose in 1991. The trends suggest that particle board and fiber board will overtake plywood.
Wood unsuitable for construction in its native form may be broken down mechanically (into fibers or chips) or chemically (into cellulose) and used as a raw material for other building materials, such as engineered wood, as well as chipboard, hardboard, and medium-density fiberboard (MDF). Such wood derivatives are widely used: wood fibers are an important component of most paper, and cellulose is used as a component of some synthetic materials. Wood derivatives can be used for kinds of flooring, for example laminate flooring.
Furniture and utensils
Wood has always been used extensively for furniture, such as chairs and beds. It is also used for tool handles and cutlery, such as chopsticks, toothpicks, and other utensils, like the wooden spoon and pencil.
Other
Further developments include new lignin glue applications, recyclable food packaging, rubber tire replacement applications, anti-bacterial medical agents, and high strength fabrics or composites. As scientists and engineers further learn and develop new techniques to extract various components from wood, or alternatively to modify wood, for example by adding components to wood, new more advanced products will appear on the marketplace. Moisture content electronic monitoring can also enhance next generation wood protection.
Art
Wood has long been used as an artistic medium. It has been used to make sculptures and carvings for millennia. Examples include the totem poles carved by North American indigenous people from conifer trunks, often Western Red Cedar (Thuja plicata).
Other uses of wood in the arts include:
- Woodcut printmaking and engraving
- Wood can be a surface to paint on, such as in panel painting
- Many musical instruments are made mostly or entirely of wood
Sports and recreational equipment
Many types of sports equipment are made of wood, or were constructed of wood in the past. For example, cricket bats are typically made of white willow. The baseball bats which are legal for use in Major League Baseball are frequently made of ash wood or hickory, and in recent years have been constructed from maple even though that wood is somewhat more fragile. National Basketball Association courts have been traditionally made out of parquetry.
Many other types of sports and recreation equipment, such as skis, ice hockey sticks, lacrosse sticks and archery bows, were commonly made of wood in the past, but have since been replaced with more modern materials such as aluminium, titanium or composite materials such as fiberglass and carbon fiber. One noteworthy example of this trend is the family of golf clubs commonly known as the woods, the heads of which were traditionally made of persimmon wood in the early days of the game of golf, but are now generally made of metal or (especially in the case of drivers) carbon-fiber composites.
Bacterial degradation
Little is known about the bacteria that degrade cellulose. Symbiotic bacteria in Xylophaga may play a role in the degradation of sunken wood. Alphaproteobacteria, Flavobacteria, Actinomycetota, Clostridia, and Bacteroidota have been detected in wood submerged for over a year.
See also
- Acetylated wood
- Ancient Chinese wooden architecture
- Ash burner
- Burl
- Carpentry
- Certified wood
- Conservation and restoration of waterlogged wood
- Conservation and restoration of wooden artifacts
- Driftwood
- Dunnage
- Forestry
- Fossil wood
- Furfurylated wood
- Green building and wood
- Helsinki Central Library Oodi
- International Wood Products Journal
- List of tallest wooden buildings
- List of woods
- Log building
- Log cabin
- Log house
- Mineral bonded wood wool board
- Mjøstårnet
- Natural building
- Parquetry
- Pallet crafts
- Pellet fuel
- Petrified wood
- Pine tar
- Plyscraper
- Pulpwood
- Reclaimed lumber
- Sawdust brandy
- Sawdust
- Thermally modified wood
- Timber framing
- Timber pilings
- Timber recycling
- Tinder
- Wood ash
- Wood degradation
- Wood drying
- Wood economy
- Wood lagging
- Wood preservation
- Wood stabilization
- Wood warping
- Wood wool
- Wood-decay fungus
- Wooden box
- Wood-plastic composite
- Woodturning
- Woodworm
- Xylology
- Xylophagy
- Xylotheque
- Xylotomy
- Yakisugi
Sources
This article incorporates text from a free content work. Licensed under CC BY-SA IGO 3.0 (license statement/permission). Text taken from World Food and Agriculture – Statistical Yearbook 2023, FAO.
References
- Hickey, M.; King, C. (2001). The Cambridge Illustrated Glossary of Botanical Terms. Cambridge University Press.
- ^ FAO. 2020. Global Forest Resources Assessment 2020: Main report Archived November 5, 2022, at the Wayback Machine. Rome.
- "The EPA Declared That Burning Wood is Carbon Neutral. It's Actually a Lot More Complicated". Archived from the original on June 30, 2021. Retrieved June 3, 2022.
- ^ Horst H. Nimz, Uwe Schmitt, Eckart Schwab, Otto Wittmann, Franz Wolf "Wood" in Ullmann's Encyclopedia of Industrial Chemistry 2005, Wiley-VCH, Weinheim. doi:10.1002/14356007.a28_305
- "N.B. fossils show origins of wood". CBC.ca. August 12, 2011. Archived from the original on August 13, 2011. Retrieved August 12, 2011.
- Philippe Gerrienne; et al. (August 12, 2011). "A Simple Type of Wood in Two Early Devonian Plants". Science. 333 (6044): 837. Bibcode:2011Sci...333..837G. doi:10.1126/science.1208882. hdl:2268/97121. PMID 21836008. S2CID 23513139.
- Woods, Sarah. "A History of Wood from the Stone Age to the 21st Century". EcoBUILDING. A Publication of The American Institute of Architects. Archived from the original on March 29, 2017. Retrieved March 28, 2017.
- Briffa, K.; Shishov, V.V.; Melvin, T.M.; Vaganov, E.A.; Grudd, H.; Hantemirov (2008). "Trends in recent temperature and radial tree growth spanning 2000 years across northwest Eurasia". Philosophical Transactions of the Royal Society B: Biological Sciences. 363 (1501): 2271–2284. doi:10.1098/rstb.2007.2199. PMC 2606779. PMID 18048299.
- Wood growth and structure Archived December 12, 2009, at the Wayback Machine www.farmforestline.com.au
- Everett, Alan; Barritt, C. M. H. (May 12, 2014). Materials. Routledge. p. 38. ISBN 978-1-317-89327-1. Archived from the original on September 8, 2023. Retrieved March 20, 2023. "Knots, particularly edge and arris knots, reduce strength mainly in tension, but not in resistance to shear and splitting."
- ^ Record, Samuel J (1914). The Mechanical Properties of Wood. J. Wiley & Sons. p. 165. ASIN B000863N3W. Archived from the original on October 18, 2020. Retrieved August 28, 2020.
- "Duramen" . Encyclopædia Britannica. Vol. 8 (11th ed.). 1911. p. 692.
- Shigo, Alex. (1986) A New Tree Biology Dictionary. Shigo and Trees, Associates. ISBN 0-943563-12-7
- Record, Samuel James (1914). The Mechanical Properties of Wood: Including a Discussion of the Factors Affecting the Mechanical Properties, and Methods of Timber Testing. J. Wiley & Sons, Incorporated. p. 51.
The term heartwood derives solely from its position and not from any vital importance to the tree as a tree can thrive with heart completely decayed.
- "Alburnum" . Encyclopædia Britannica. Vol. 1 (11th ed.). 1911. p. 516.
- Capon, Brian (2005), Botany for Gardeners (2nd ed.), Portland, OR: Timber Publishing, p. 65 ISBN 0-88192-655-8
- "Wood Properties Growth and Structure 2015". treetesting.com. Archived from the original on March 13, 2016.
- "Timber Plus Toolbox, Selecting timber, Characteristics of timber, Structure of hardwoods". nationalvetcontent.edu.au. Archived from the original on August 10, 2014.
- ^ Sperry, John S.; Nichols, Kirk L.; Sullivan, June E.; Eastlack, Sondra E. (1994). "Xylem Embolism in ring-porous, diffuse-porous, and coniferous trees of Northern Utah and Interior Alaska" (PDF). Ecology. 75 (6): 1736–1752. Bibcode:1994Ecol...75.1736S. doi:10.2307/1939633. JSTOR 1939633. Archived from the original (PDF) on August 10, 2017. Retrieved November 30, 2018.
- Record, Samuel James (1914). The Mechanical Properties of Wood, Including a Discussion of the Factors Affecting the Mechanical Properties, and Methods of Timber Testing. J. Wiley & sons, Incorporated. Archived from the original on September 8, 2023. Retrieved March 20, 2023.
- ^ Samuel James Record (1914). The mechanical properties of wood, including a discussion of the factors affecting the mechanical properties, and methods of timber testing. J. Wiley & sons, inc. pp. 44–.
- ^ U.S. Department of Agriculture, Forest Products Laboratory. The Wood Handbook: Wood as an engineering material Archived March 15, 2007, at the Wayback Machine. General Technical Report 113. Madison, WI.
- ^ Timell, T.E. 1986. Compression wood in gymnosperms. Springer-Verlag, Berlin. 2150 p.
- "Wood Handbook: Chapter 4: Moisture Relations and Physical Properties of Wood" (PDF). U.S. Forest Products Laboratory. Archived (PDF) from the original on December 30, 2023. Retrieved September 10, 2023.
- "Standard Practice for Establishing Clear Wood Strength Values". www.astm.org. Archived from the original on April 1, 2023. Retrieved September 9, 2023.
- Elliott, G.K. 1970. Wood density in conifers. Commonwealth For. Bureau, Oxford, U.K., Tech. Commun. 8. 44 p.
- Green, D.W.; Winandy, J.E.; Kretschmann, D.E. (1999). "4. Mechanical Properties of Wood" (PDF). Wood handbook: Wood as an engineering material (Technical report). U.S. Department of Agriculture, Forest Service, Forest Products Laboratory. p. 463. doi:10.2737/FPL-GTR-113. hdl:2027/mdp.39015000158041. FPL–GTR–113.
- ^ "PFAF". pfaf.org. Archived from the original on October 24, 2019. Retrieved November 3, 2019.
- "What are the mechanical properties of bamboo". www.DoorStain.com. August 22, 2023. Archived from the original on August 22, 2023. Retrieved August 22, 2023.
- Agriculture Handbook. U.S. Department of Agriculture. 1997. pp. 2–6. Archived from the original on September 8, 2023. Retrieved March 20, 2023.
- Jean-Pierre Barette; Claude Hazard et Jérôme Mayer (1996). Mémotech Bois et Matériaux Associés. Paris: Éditions Casteilla. p. 22. ISBN 978-2-7135-1645-0.
- W. Boerjan; J. Ralph; M. Baucher (June 2003). "Lignin biosynthesis". Annu. Rev. Plant Biol. 54 (1): 519–549. doi:10.1146/annurev.arplant.54.031902.134938. PMID 14503002.
- ^ Ek, Monica; Gellerstedt, Göran; Henriksson, Gunnar (2009). "Chapter 7: Wood extractives". Pulp and Paper Chemistry and Technology. Volume 1, Wood Chemistry and Wood Biotechnology. Berlin: Walter de Gruyter. ISBN 978-3-11-021339-3.
- ^ Sjöström, Eero (October 22, 2013). "Chapter 5: Extractives". Wood Chemistry: Fundamentals and Applications (Second ed.). San Diego: Elsevier Science. ISBN 978-0-08-092589-9.
- Ansell, Martin P. (2015). "Chapter 11: Preservation, Protection and Modification of Wood Composites". Woodhead Publishing Series in Composites Science and Engineering: Number 54. Wood Composites. Cambridge, UK: Woodhead Publishing. ISBN 978-1-78242-454-3.
- ^ Hon, David N.-S.; Shiraishi, Nubuo (2001). "Chapter 6: Chemistry of Extractives". Wood and Cellulosic Chemistry (2nd, rev. and expanded ed.). New York: Marcel Dekker. ISBN 0-8247-0024-4.
- Rowell, Roger M. (2013). "Chater 3: Cell Wall Chemistry". Handbook of Wood Chemistry and Wood Composites (2nd ed.). Boca Raton: Taylor & Francis. ISBN 9781439853801.
- Mimms, Agneta; Michael J. Kuckurek; Jef A. Pyiatte; Elizabeth E. Wright (1993). Kraft Pulping. A Compilation of Notes. TAPPI Press. pp. 6–7. ISBN 978-0-89852-322-5.
- Fiebach, Klemens; Grimm, Dieter (2000). "Resins, Natural". Ullmann's Encyclopedia of Industrial Chemistry. doi:10.1002/14356007.a23_073. ISBN 978-3-527-30673-2.
- Sperelakis, Nicholas; Sperelakis, Nick (January 11, 2012). "Chapter 4: Ionophores in Planar Lipid Bilayers". Cell physiology sourcebook: essentials of membrane biophysics (Fourth ed.). London, UK. ISBN 978-0-12-387738-3. Archived from the original on June 28, 2020. Retrieved September 27, 2020.
{{cite book}}
: CS1 maint: location missing publisher (link) - Saniewski, Marian; Horbowicz, Marcin; Kanlayanarat, Sirichai (September 10, 2014). "The Biological Activities of Troponoids and Their Use in Agriculture A Review". Journal of Horticultural Research. 22 (1): 5–19. doi:10.2478/johr-2014-0001. S2CID 33834249.
- Bentley, Ronald (2008). "A fresh look at natural tropolonoids". Nat. Prod. Rep. 25 (1): 118–138. doi:10.1039/b711474e. PMID 18250899.
- World Food and Agriculture – Statistical Yearbook 2023. FAO. November 29, 2023. doi:10.4060/cc8166en. ISBN 978-92-5-138262-2.
- Sterrett, Frances S. (October 12, 1994). Alternative Fuels and the Environment. CRC Press. ISBN 978-0-87371-978-0. Archived from the original on December 30, 2023. Retrieved October 6, 2020.
- "Saitta House – Report Part 1 Archived December 16, 2008, at the Wayback Machine",DykerHeightsCivicAssociation.com
- Binggeli, Corky (2013). Materials for Interior Environments. John Wiley & Sons. ISBN 978-1-118-42160-4. Archived from the original on December 30, 2023. Retrieved October 6, 2020.
- ^ "APA – The Engineered Wood Association" (PDF). apawood.org. Archived (PDF) from the original on June 27, 2006.
- "FPInnovations" (PDF). forintek.ca. Archived from the original (PDF) on March 19, 2009.
- "System for remotely monitoring moisture content on wooden elements" I Arakistain, O Munne EP Patent EPO1382108.0
- Christina Bienhold; Petra Pop Ristova; Frank Wenzhöfer; Thorsten Dittmar; Antje Boetius (January 2, 2013). "How Deep-Sea Wood Falls Sustain Chemosynthetic Life". PLOS ONE. 8 (1): e53590. Bibcode:2013PLoSO...853590B. doi:10.1371/journal.pone.0053590. PMC 3534711. PMID 23301092.
- Hoadley, R. Bruce (2000). Understanding Wood: A Craftsman's Guide to Wood Technology. Taunton Press. ISBN 978-1-56158-358-4.
External links
- The Wood in Culture Association (archived 27 May 2016)
- The Wood Explorer: A comprehensive database of commercial wood species (Archived April 7, 2015, at the Wayback Machine)
- APA – The Engineered Wood Association (archived 14 April 2011)
Botany | |||||||||||
---|---|---|---|---|---|---|---|---|---|---|---|
Subdisciplines | |||||||||||
Plant groups | |||||||||||
Plant anatomy |
| ||||||||||
Plant physiology Materials | |||||||||||
Plant growth and habit | |||||||||||
Reproduction | |||||||||||
Plant taxonomy | |||||||||||
Practice | |||||||||||
| |||||||||||
Wood products | |
---|---|
Lumber/ timber | |
Engineered wood | |
Fuelwood | |
Fibers | |
Derivatives | |
By-products | |
Historical | |
See also | |
Natural resources | |||||||
---|---|---|---|---|---|---|---|
Air |
| ||||||
Energy | |||||||
Land | |||||||
Life | |||||||
Water |
| ||||||
Related |
| ||||||
Sources of tannins | |||||||||||||||||
---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
Sources of condensed tannins |
| ||||||||||||||||
Sources of hydrolysable tannins |
| ||||||||||||||||
Other sources by organ |
|
Sculpture | |
---|---|
Types of sculpture | |
Styles of sculpture | |
Elements in sculpture | |
Traditional materials | |
Modern materials | |
Notable sculptures |
|